(19)
(11)EP 3 555 332 B1

(12)EUROPEAN PATENT SPECIFICATION

(45)Mention of the grant of the patent:
26.01.2022 Bulletin 2022/04

(21)Application number: 17830056.2

(22)Date of filing:  12.12.2017
(51)International Patent Classification (IPC): 
C22C 21/08(2006.01)
C22F 1/05(2006.01)
(52)Cooperative Patent Classification (CPC):
C22C 21/08; C22F 1/002; C22C 21/04; C22F 1/05
(86)International application number:
PCT/US2017/065715
(87)International publication number:
WO 2018/111813 (21.06.2018 Gazette  2018/25)

(54)

HIGH STRENGTH AND HIGHLY FORMABLE ALUMINUM ALLOYS RESISTANT TO NATURAL AGE HARDENING AND METHODS OF MAKING THE SAME

HOCHFESTE UND HOCHVERFORMBARE ALUMINIUMLEGIERUNGEN, DIE GEGEN NATÜRLICHE ALTERSHÄRTUNG RESISTENT SIND, UND VERFAHREN ZUR HERSTELLUNG DAVON

ALLIAGES D'ALUMINIUM DE HAUTE RÉSISTANCE ET DE HAUTE APTITUDE AU FORMAGE RÉSISTANCE AU DURCISSEMENT PAR VIEILLISSEMENT NATUREL ET SES PROCÉDÉS DE FABRICATION


(84)Designated Contracting States:
AL AT BE BG CH CY CZ DE DK EE ES FI FR GB GR HR HU IE IS IT LI LT LU LV MC MK MT NL NO PL PT RO RS SE SI SK SM TR

(30)Priority: 16.12.2016 US 201662435382 P
28.03.2017 US 201762477677 P

(43)Date of publication of application:
23.10.2019 Bulletin 2019/43

(73)Proprietor: Novelis Inc.
Atlanta, GA 30326 (US)

(72)Inventors:
  • FLOREY, Guillaume
    3968 Veyras (CH)
  • BASSI, Corrado
    3970 Salgesch (CH)
  • DESPOIS, Aude
    3979 Grone (CH)
  • LEYVRAZ, David
    3960 Sierre (CH)

(74)Representative: Weickmann & Weickmann PartmbB 
Postfach 860 820
81635 München
81635 München (DE)


(56)References cited: : 
EP-A1- 2 987 879
WO-A1-02/090608
  
  • GUO M X ET AL: "Enhanced bake-hardening response of an Al-Mg-Si-Cu alloy with", MATERIALS CHEMISTRY AND PHYSICS, vol. 162, 2015, pages 15-19, XP029251788, ISSN: 0254-0584, DOI: 10.1016/J.MATCHEMPHYS.2015.07.033
  • CHIN-HUI SHEN: "Pre-treatment to Improve the Bake-hardening Response in the Naturally Aged Al-Mg-Si Alloy", JOURNAL OF MATERIALS SCIENCE & TECHNOLOGY, vol. 27, no. 3, 1 January 2011 (2011-01-01), pages 205-212, XP055450124, AMSTERDAM, NL ISSN: 1005-0302, DOI: 10.1016/S1005-0302(11)60050-9
  • ZHUANG L ET AL: "IMPROVEMENT IN BAKE HARDENING RESPONSE OF AL-SI-MG ALLOYS", MATERIALS SCIENCE FORUM, TRANS TECH PUBLICATIONS LTD- SWITZERLAND, CH, vol. 331-337, 1 January 2000 (2000-01-01), pages 1309-1314, XP001154767, ISSN: 0255-5476
  
Note: Within nine months from the publication of the mention of the grant of the European patent, any person may give notice to the European Patent Office of opposition to the European patent granted. Notice of opposition shall be filed in a written reasoned statement. It shall not be deemed to have been filed until the opposition fee has been paid. (Art. 99(1) European Patent Convention).


Description

CROSS-REFERENCE TO RELATED APPLICATIONS



[0001] This application claims the benefit of U.S. Provisional Application Nos. 62/435,382, filed December 16, 2016, and 62/477,677, filed March 28, 2017.

FIELD



[0002] This disclosure relates to high-strength aluminum alloys and methods of making and processing the same. The disclosure further relates to heat treatable aluminum alloys exhibiting improved mechanical strength and formability.

BACKGROUND



[0003] Recyclable aluminum alloys with high strength are desirable for improved product performance in many applications, including transportation (encompassing without limitation, e.g., trucks, trailers, trains, and marine) applications, electronics applications, automobile applications and others. For example, a high-strength aluminum alloy in trucks or trailers would be lighter than conventional steel alloys, which may provide significant emission reductions that are needed to meet new, stricter government regulations on emissions. Such alloys should exhibit high strength, high formability, and corrosion resistance.

[0004] EP 2 987 879 A1 discloses an aluminum alloy material suitable for manufacturing of automobile sheet and a preparation method thereof.

[0005] Chin-Hui Shen, Pre-treatment to Improve the Bake-hardening Response in the Naturally Aged Al-Mg-Si Alloy, J. Mater. Sci. Technol., 2011, 27(3), 205-212 describes pre-treatment methods to improve the bake hardening response of naturally aged AA6022, which is an alloy used in automotive body panels.

[0006] M.X. Guo et al., Enhanced bake-hardening response of an Al-Mg-Si-Cu alloy with Zn addition, Materials Chemistry and Physics 162 (2015), 15-19, reports that Zn addition greatly enhances the bake-hardening response of an Al-Mg-Si-Cu alloy.

[0007] WO 02/090608 A1 describes a process for preparing an aluminum alloy sheet with improved bendability and an aluminum alloy sheet produced therefrom.

SUMMARY



[0008] The present invention relates to a method of producing an aluminum alloy metal product, the method comprising;

casting an aluminum alloy to form a cast aluminum alloy product, wherein the aluminum alloy comprises 0.25 - 1.1 wt. % Cu, 0.6 - 1.1 wt. % Si, 0.7 - 1.2 wt. % Mg, up to 0.25 wt. % Cr, up to 0.35 wt. % Mn, up to 0.4 wt. % Fe, up to 0.25 wt. % Zr, from 0.06 to 0.3 wt. % Zn, up to 0.30 wt. % Ti, up to 0.04 wt. % Ni, and up to 0.15 wt. % of impurities, with the remainder as Al;

homogenizing the cast aluminum alloy product by heating to a temperature from 520°C to 580°C with a soaking time from 30 minutes to 18 hours;

hot rolling the cast aluminum alloy product to produce a sheet, plate, or shate with a hot mill entry temperature of 440°C to 540°C and a hot roll exit temperature of 250°C to 380°C; solutionizing the sheet, plate, or shate at a temperature between 520 °C and 580 °C and then quenching at a quench rate from 50°C/s to 400°C/s;

pre-aging the sheet, plate, or shate, wherein the pre-aging comprises heating the sheet, plate or shate to a pre-aging temperature of 115°C to 135°C after solutionizing and soaking at the pre-aging temperature for a period of time; and

coiling the sheet, plate, or shate.



[0009] The invention further relates to an aluminum alloy metal product, wherein the aluminum alloy metal product is prepared by the inventive method.

[0010] Covered embodiments of the invention are defined by the claims, not this summary. This summary is a high-level overview of various aspects of the invention and introduces some of the concepts that are further described in the Detailed Description section below. This summary is not intended to identify key or essential features of the claimed subject matter, nor is it intended to be used in isolation to determine the scope of the claimed subject matter. The subject matter should be understood by reference to appropriate portions of the entire specification, any or all drawings and each claim.

[0011] Provided herein are methods of preparing 6xxx series aluminum alloys, the aluminum alloys, and products comprising the disclosed alloys.

[0012] One aspect relates to methods of processing aluminum. For example, disclosed herein are methods of producing an aluminum alloy product, the method comprising casting an aluminum alloy to form a cast aluminum alloy product, wherein the aluminum alloy comprises 0.25 - 1.1 wt. % Cu, 0.6 - 1.1 wt. % Si, 0.7 - 1.2 wt. % Mg, up to 0.25 wt. % Cr, up to 0.35 wt. % Mn, up to 0.4 wt. % Fe, up to 0.25 wt. % Zr, from 0.06 to 0,3 wt. % Zn, up to 0.10 wt. % Ti, up to 0.04 wt. % Ni, and up to 0.15 wt. % of impurities, with the remainder as Al; homogenizing the cast aluminum alloy product; hot rolling the cast aluminum alloy product to produce a rolled product (e.g., a sheet, a plate, or a shate); solutionizing the sheet, plate, or shate at a temperature between 520 °C and 580 °C; pre-aging the sheet, plate, or shate; and coiling the aluminum alloy sheet, plate, or shate. Throughout this application, all elements are described in weight percentage (wt. %) based on the total weight of the alloy.

[0013] In some examples, the aluminum alloy can include 0.6 - 1.1 wt. % Cu, 0.6 - 1.1 wt. % Si, 0.7 - 1.2 wt. % Mg, up to 0.25 wt. % Cr, up to 0.35 wt. % Mn, 0.05 - 0.4 wt. % Fe, up to 0.25 wt. % Zr, from 0.06 to 0.3 wt. % Zn, up to 0.10 wt. % Ti, up to 0.04 wt. % Ni, and up to 0.15 wt. % of impurities, with the remainder as Al. In some cases, the aluminum alloy can include 0.7 - 1.0 wt. % Cu, 0.65 - 1.0 wt. % Si, 0.8 - 1.1 wt. % Mg, 0.01 - 0.20 wt. % Cr, up to 0.25 wt. % Mn, 0.10 - 0.35 wt. % Fe, up to 0.2 wt. % Zr, from 0.06 to 0.2 wt. % Zn, 0.01 - 0.05 wt. % Ti, up to 0.035 wt. % Ni, and up to 0.15 wt. % of impurities, with the remainder as Al. In some cases, the aluminum alloy can include 0.75 - 0.9 wt. % Cu, 0.65 - 0.9 wt. % Si, 0.85 - 1.0 wt. % Mg, 0.05 - 0.18 wt. % Cr, 0.05 - 0.18 wt. % Mn, 0.12 - 0.30 wt. % Fe, up to 0.15 wt. % Zr, from 0.06 to 0.1 wt. % Zn, 0.01 - 0.04 wt. % Ti, up to 0.034 wt. % Ni, and up to 0.15 wt. % of impurities, with the remainder as Al.

[0014] The pre-aging the sheet, plate, or shate step comprises heating the sheet, plate, or shate to a temperature of 115 °C to 135 °C, or in some cases between 120 °C to 130 °C, after solutionizing. In some aspects, the pre-aging step after the solutionizing step can provide an aluminum alloy in a pre-aged condition resulting in an exemplary temper that can exhibit improved resistance to natural aging of the alloy and/or improved uniform formability. In some cases, a pre-aged alloy resistant to natural age-hardening can exhibit an increased shelf life for storing as-produced aluminum alloys.

[0015] The methods described herein can further comprise strain hardening and/or thermal treating the aluminum alloy product. The strain hardening can optionally be performed at 2 % and the thermal treating can comprise maintaining the aluminum alloy product at a temperature of 185 °C for a time period of 20 minutes.

[0016] The methods described herein further comprise quenching the aluminum alloy product after the solutionizing step; cold rolling the aluminum alloy product; aging the aluminum alloy product (e.g., by heating the aluminum alloy product between 180 °C to 225 °C for a period of time); and/or pre-straining the aluminum metal product, wherein the pre-straining comprises applying a tensile strain to the aluminum alloy product after solutionizing.

[0017] Optionally, the aluminum alloy product comprises a strain hardening exponent of at least 0.23. Optionally, the aluminum alloy product comprises a strength of at least 300 MPa after a 2% pre-strain hardening and thermal treatment of 185 °C for a time period of 20 minutes. In some non-limiting examples, the aluminum alloy product comprises a strength of at least 300 MPa.

[0018] Also disclosed are aluminum alloy products (e.g., transportation body parts, such as automotive body parts or structural body parts, and electronics device housings) comprising an alloy obtained according to the methods provided herein.

[0019] Further aspects, objects, and advantages will become apparent upon consideration of the detailed description of non-limiting examples and figures that follow.

BRIEF DESCRIPTION OF THE DRAWINGS



[0020] 

Figure 1 is a graph showing a comparison between the tensile properties over time of an exemplary alloy exposed to various pre-aging conditions after solutionizing.

Figure 2 is a graph showing a comparison between the elongation over time of an exemplary alloy exposed to various pre-aging conditions after solutionizing.

Figure 3 is a graph showing a comparison between the paint bake response of an exemplary alloy exposed to various pre-aging conditions after solutionizing.

Figure 4 is a graph showing a comparison between the coil cooling rates of an exemplary alloy exposed to various pre-aging conditions after solutionizing.

Figure 5 is a graph showing the temperature coil cooling rates of a comparative aluminum alloy at various positions over the coil diameter after pre-aging.

Figure 6 is a graph showing a comparison of yield strength stability over time of an exemplary alloy in T4 temper at various positions over the coil diameter.

Figure 7 is a graph showing a comparison of paint bake response stability over time of an exemplary alloy at various positions over the coil diameter.

Figure 8 is a graph showing a comparison of elongation stability over time of an exemplary alloy at various positions over the coil diameter.

Figure 9 is a graph showing natural age hardening of a comparative alloy subjected to a pre-aging temperature of 100 °C after solutionizing.

Figure 10 is a graph showing natural age hardening of an exemplary alloy subjected to a pre-aging temperature of 130 °C after solutionizing.

Figure 11 is a graph showing a comparison of in-service yield strength of an exemplary alloy in an exemplary temper subjected to various pre-aging temperatures after solutionizing.

Figure 12 is a graph showing a comparison of paint bake response over time of an exemplary alloy subjected to various pre-aging temperatures after solutionizing.

Figure 13 is a graph showing a comparison of n-value of an exemplary alloy subjected to various pre-aging temperatures after solutionizing.

Figure 14 is a graph showing a comparison of yield strength stability over time of an exemplary alloy subjected to various pre-aging temperatures after solutionizing.

Figure 15 is a graph showing the aging difference of yield strength (Rp02) after 1 month of aging of an exemplary alloy subjected to various pre-aging temperatures after solutionizing.

Figure 16 is a graph showing the outer bending angle normalized to 2.0 mm according to the VDA 238-100 test specification of an exemplary alloy over time in T6 temper subjected to various pre-aging temperatures after solutionizing.

Figure 17 is a graph showing a comparison of strain hardening exponent (n-value (n10-20)) over time of an exemplary alloy subjected to various pre-aging temperatures after solutionizing.

Figure 18 is a graph showing a comparison of elongation (Ag) over time of an exemplary alloy and a comparative alloy.

Figure 19 is a graph showing the yield strength of a comparative alloy after various pre-aging temperatures.

Figure 20 is a graph showing the yield strength of a comparative alloy after various pre-aging temperatures.

Figure 21 is a graph showing the yield strength of a comparative alloy after various pre-aging temperatures.

Figure 22A is a graph showing a comparison of bake hardening (BH) over time of a comparative alloy.

Figure 22B is a graph showing a comparison of bake hardening (BH) over time of a comparative alloy.

Figure 22C is a graph showing a comparison of bake hardening (BH) over time of a comparative alloy.

Figure 22D is a graph showing a comparison of bake hardening (BH) over time of an exemplary alloy.

Figure 23 is a graph showing a comparison of yield strength over time of an exemplary alloy in a T4 temper and comparative alloys in a T4 temper.

Figure 24 is a graph showing a comparison of formability over time of an exemplary alloy and comparative alloys.

Figure 25 is a graph showing a comparison of yield strength over time of an exemplary alloy in a T8x temper and comparative alloys in a T8x temper.

Figure 26A is a graph showing yield strength after natural aging of an exemplary alloy.

Figure 26B is a graph showing yield strength after paint baking and natural aging of an exemplary alloy.

Figure 27 is a schematic diagram of a process as described herein.

Figure 28 is a graph showing the bend angles and strength for aluminum alloys subjected to various pre-straining procedures.

Figure 29 is a graph showing the percent elongation and strength for aluminum alloys subjected to various pre-straining procedures.

Figure 30 is a graph showing the yield strengths of aluminum alloys subjected to various pre-straining procedures as described herein upon delivery to a customer and after post-forming heat treatment (PFHT).

Figure 31 is a graph showing the tensile strengths of aluminum alloys subjected to various pre-straining procedures as described herein upon delivery to a customer and after post-forming heat treatment (PFHT).

Figure 32 is a graph showing the percent elongation values of aluminum alloys subjected to various pre-straining procedures as described herein upon delivery to a customer and after post-forming heat treatment (PFHT).

Figure 33 is a graph showing the bend angles of aluminum alloys subjected to various pre-straining procedures as described herein upon delivery to a customer and after post-forming heat treatment (PFHT).

Figure 34 is a graph showing the bend angles and strength for aluminum alloys subjected to various pre-straining procedures.

Figure 35 is a graph showing the percent elongation and strength for aluminum alloys subjected to various pre-straining procedures.

Figure 36 is a graph showing the yield strengths of aluminum alloys subjected to a pre-straining procedure as described herein upon delivery to a customer and after various paint baking heat treatments.

Figure 37 is a graph showing the percent elongation values of aluminum alloys subjected to a pre-straining procedure as described herein upon delivery to a customer and after various paint baking heat treatments.


DETAILED DESCRIPTION



[0021] Described herein are heat treatable aluminum alloys and methods of making and processing the same. The heat treatable aluminum alloys exhibit improved mechanical strength and deformability properties, including formability and bendability. The alloys can be processed in a method such that the resulting metal products have high strength and high deformability properties. The properties of the metal products can be further enhanced during downstream processing (e.g., end user forming and post-forming heat treating the metal product, or end user paint baking). Surprisingly, due to the conditions used during the processing methods as further described herein, the metal products can achieve an increased final strength without degrading the final bendability or elongation.

Definitions and Descriptions



[0022] The terms "invention," "the invention," "this invention" and "the present invention" used herein are intended to refer broadly to all of the subject matter of this patent application and the claims below. Statements containing these terms should be understood not to limit the subject matter described herein or to limit the meaning or scope of the patent claims below.

[0023] In this description, reference is made to alloys identified by aluminum industry designations, such as "series" or "6xxx." For an understanding of the number designation system most commonly used in naming and identifying aluminum and its alloys, see "International Alloy Designations and Chemical Composition Limits for Wrought Aluminum and Wrought Aluminum Alloys" or "Registration Record of Aluminum Association Alloy Designations and Chemical Compositions Limits for Aluminum Alloys in the Form of Castings and Ingot," both published by The Aluminum Association.

[0024] As used herein, the meaning of "a," "an," or "the" includes singular and plural references unless the context clearly dictates otherwise.

[0025] As used herein, the meaning of "room temperature" can include a temperature of from 15 °C to 30 °C, for example 15 °C, 16 °C, 17 °C, 18 °C, 19 °C, 20 °C, 21 °C, 22 °C, 23 °C, 24 °C, 25 °C, 26 °C, 27 °C, 28 °C, 29 °C, or 30 °C.

[0026] As used herein, a "plate" generally has a thickness of greater than 15 mm. For example, a plate may refer to an aluminum product having a thickness of greater than 15 mm, greater than 20 mm, greater than 25 mm, greater than 30 mm, greater than 35 mm, greater than 40 mm, greater than 45 mm, greater than 50 mm, or greater than 100 mm.

[0027] As used herein, a "shate" (also referred to as a sheet plate) generally refers to an aluminum product having a thickness of from 4 mm to 15 mm. For example, a shate may have a thickness of 4 mm, 5 mm, 6 mm, 7 mm, 8 mm, 9 mm, 10 mm, 11 mm, 12 mm, 13 mm, 14 mm, or 15 mm.

[0028] As used herein, a "sheet" generally refers to an aluminum product having a thickness of less than 4 mm. For example, a sheet may have a thickness of less than 4 mm, less than 3 mm, less than 2 mm, less than 1 mm, less than 0.5 mm, less than 0.3 mm, or less than0.1 mm.

[0029] As used herein, terms such as "cast aluminum alloy product," "cast product," and the like are interchangeable and refer to a product produced by direct chill casting (including direct chill co-casting) or semi-continuous casting, continuous casting (including, for example, by use of a twin belt caster, a twin roll caster, a block caster, or any other continuous caster), electromagnetic casting, hot top casting, or any other casting method. All ranges disclosed herein are to be understood to encompass any and all subranges subsumed therein. For example, a stated range of "1 to 10" should be considered to include any and all subranges between (and inclusive of) the minimum value of 1 and the maximum value of 10; that is, all subranges beginning with a minimum value of 1 or more, e.g. 1 to 6.1, and ending with a maximum value of 10 or less, e.g., 5.5 to 10.

[0030] Reference is made in this application to alloy temper or condition. For an understanding of the alloy temper descriptions most commonly used, see "American National Standards (ANSI) H35 on Alloy and Temper Designation Systems." An F condition or temper refers to an aluminum alloy as fabricated. An O condition or temper refers to an aluminum alloy after annealing. A T3 condition or temper refers to an aluminum alloy solution heat treated (i.e., solutionized), cold worked, and naturally aged. A T4 condition or temper refers to an aluminum alloy solution heat treated and naturally aged. A T6 condition or temper refers to an aluminum alloy solution heat treated and artificially aged. A T8x condition or temper refers to an aluminum alloy solution heat treated, cold worked, and artificially aged.

[0031] The following aluminum alloys are described in terms of their elemental composition in weight percentage (wt. %) based on the total weight of the alloy. In certain examples of each alloy, the remainder is aluminum, with a maximum wt. % of 0.15 % for the sum of the impurities.

Alloy Composition



[0032] Described herein are novel aluminum alloys that can exhibit high strength and high formability. In some cases, the aluminum alloys include heat treatable aluminum alloys. As used herein, heat treatable aluminum alloys include 2xxx series alloys, 6xxx series alloys, and 7xxx series alloys. In certain aspects, the alloys exhibit high strength and high deformability. In some cases, the alloys exhibit an increase in strength after thermal treatment without significant loss of deformability. The properties of the alloys are achieved at least in part due to the methods of processing the alloys to produce the described plates, shates, sheets or other products.

[0033] In some examples, the alloys can have the following elemental composition as provided in Table 1.
Table 1
ElementWeight Percentage (wt. %)
Cu 0.25 - 1.1
Si 0.6 - 1.1
Mg 0.7 - 1.2
Cr 0.0 - 0.25
Mn 0.0 - 0.35
Fe 0.0 - 0.4
Zr 0.0 - 0.25
Zn 0.06 - 0.3
Ti 0.0 - 0.3
Ni 0.0 - 0.04
Impurities 0.0 - 0.05 (each) 0.0 - 0.15 (total)
Al Remainder


[0034] In some examples, the alloys can have the following elemental composition as provided in Table 2.
Table 2
ElementWeight Percentage (wt. %)
Cu 0.6 - 1.1
Si 0.6 - 1.1
Mg 0.7 - 1.2
Cr 0.0 - 0.25
Mn 0.0 - 0.35
Fe 0.05 - 0.4
Zr 0.0 - 0.25
Zn 0.06 - 0.3
Ti 0.0-0.10
Ni 0.0 - 0.04
Impurities 0.0 - 0.05 (each)
0.0 - 0.15 (total)
Al Remainder


[0035] In other examples, the alloys can have the following elemental composition as provided in Table 3.
Table 3
ElementWeight Percentage (wt. %)
Cu 0.7 - 1.0
Si 0.65 - 1.0
Mg 0.8 - 1.1
Cr 0.01 - 0.20
Mn 0.0 - 0.25
Fe 0.10-0.35
Zr 0.0 - 0.2
Zn 0.06 - 0.2
Ti 0.01 - 0.07
Ni 0.0 - 0.034
Impurities 0.0 - 0.05 (each)
0.0 - 0.15 (total)
Al Remainder


[0036] In one example, an aluminum alloy can have the following elemental composition as provided in Table 4. In certain aspects, the alloy is used to prepare aluminum plates and shates.
Table 4
ElementWeight Percentage (wt. %)
Cu 0.75 - 0.9
Si 0.65 - 0.9
Mg 0.85 - 1.0
Cr 0.05 - 0.18
Mn 0.05 - 0.18
Fe 0.12 - 0.30
Zr 0.0-0.15
Zn 0.06 - 0.15
Ti 0.012 - 0.05
Ni 0.0 - 0.034
Impurities 0.0 - 0.05 (each)
0.0 - 0.15 (total)
Al Remainder


[0037] In certain examples, the disclosed alloy includes copper (Cu) in an amount from 0.25 % to 1.1 % (e.g., from 0.6 % to 1.1 %, from 0.65 % to 0.9 %, from 0.7 % to 1.0 %, or from 0.6 % to 0.7 %) based on the total weight of the alloy. For example, the alloys can include 0.25 %,0.26 %, 0.27 %, 0.28 %, 0.29 %, 0.3 %,0.31%, 0.32 %, 0.33 %, 0.34 %,0.35 %, 0.36 %, 0.37 %,0.38 %, 0.39 %,0.4 %,0.41 %, 0.42 %,0.43 %,0.44 %, 0.45 %, 0.46 %, 0.47 %, 0.48 %, 0.49 %, 0.5 %, 0.51 %, 0.52 %, 0.53 %, 0.54 %, 0.55 %, 0.56 %, 0.57 %,0.58 %, 0.59 %, 0.6 %, 0.61 %, 0.62 %, 0.63 %, 0.64 %, 0.65 %, 0.66 %, 0.67 %, 0.68 %, 0.69 %, 0.7 %, 0.71 %, 0.72 %, 0.73 %, 0.74 %, 0.75 %, 0.76 %, 0.77 %, 0.78 %, 0.79 %,0.8 %, 0.81 %, 0.82 %, 0.83 %, 0.84 %, 0.85 %, 0.86 %, 0.87 %, 0.88 %, 0.89 %, 0.9 %,0.91 %, 0.92 %, 0.93 %, 0.94 %, 0.95 %, 0.96 %, 0.97 %, 0.98 %, 0.99 %, 1.0 %, 1.01 %, 1.02 %, 1.03 %, 1.04 %, 1.05 %, 1.06 %, 1.07 %, 1.08 %, 1.09 %, or 1.1 % Cu. All expressed in wt. %.

[0038] In certain examples, the disclosed alloy includes silicon (Si) in an amount from 0.6 % to 1.1 % (e.g., from 0.65 % to 1.0 %, from 0.9 % to 1.1 %, from 0.65 % to 0.9 %, from 0.9 % to 1.1 %, or from 1.0 % to 1.1 %) based on the total weight of the alloy. For example, the alloys can include 0.6 %, 0.61 %, 0.62 %, 0.63 %, 0.64 %, 0.65 %, 0.66 %, 0.67 %, 0.68 %, 0.69 %, 0.7 %, 0.71 %, 0.72 %, 0.73 %, 0.74 %, 0.75 %, 0.76 %, 0.77 %, 0.78 %, 0.79 %, 0.8 %, 0.81 %, 0.82 %, 0.83 %, 0.84 %, 0.85 %, 0.86 %, 0.87 %, 0.88 %, 0.89 %, 0.9 %, 0.91 %, 0.92 %, 0.93 %, 0.94 %, 0.95 %, 0.96 %, 0.97 %, 0.98 %, 0.99 %, 1.0 %, 1.01 %, 1.02 %, 1.03 %, 1.04 %, 1.05 %, 1.06 %, 1.07 %, 1.08 %, 1.09 %, or 1.1 % Si. All expressed in wt. %.

[0039] In certain examples, the disclosed alloy includes magnesium (Mg) in an amount from 0.7 % to 1.2 % (e.g., from 1.0 % to 1.25 %, from 1.1 % to 1.25 %, from 1.1 % to 1.2 %, from 1.0 % to 1.2 %, from 1.05 % to 1.3 %, or from 1.15 % to 1.3 %) based on the total weight of the alloy. For example, the alloys can include 0.7 %, 0.71 %, 0.72 %, 0.73 %, 0.74 %, 0.75 %, 0.76 %, 0.77 %, 0.78 %, 0.79 %, 0.8 %, 0.81 %, 0.82 %, 0.83 %, 0.84 %, 0.85 %, 0.86 %, 0.87 %, 0.88 %, 0.89 %, 0.9 %, 0.91 %, 0.92 %, 0.93 %, 0.94 %, 0.95 %, 0.96 %, 0.97 %, 0.98 %, 0.99 %, 1.0 %, 1.01 %, 1.02 %, 1.03 %, 1.04 %, 1.05 %, 1.06 %, 1.07 %, 1.08 %, 1.09 %, 1.1 %, 1.11 %, 1.12 %, 1.13 %, 1.14 %, 1.15 %, 1.16 %, 1.17 %, 1.18 %, 1.19 %, or 1.2 % Mg. All expressed in wt. %.

[0040] In certain aspects, for a combined effect of strengthening and, the alloy has a Cu content of less than 0.72 wt. % along with a controlled Si to Mg ratio of 1.11:1.

[0041] In certain aspects, the alloy includes chromium (Cr) in an amount up to 0.25 % (e.g., from 0.03 % to 0.06 %, from 0.03 % to 0.19 %, or from 0.06 % to 0.1 %) based on the total weight of the alloy. For example, the alloy can include 0.001 %, 0.002 %, 0.003 %, 0.004 %, 0.005 %, 0.006 %, 0.007 %, 0.008 %, 0.059 %, 0.01 %, 0.011 %, 0.012 %, 0.013 %, 0.014 %, 0.015 %, 0.016 %, 0.017 %, 0.018 %, 0.019 %, 0.02 %, 0.021 %, 0.022 %, 0.023 %, 0.024 %, 0.025 %, 0.026 %, 0.027 %, 0.028 %, 0.029 %, 0.03 %, 0.031 %, 0.032 %, 0.033 %, 0.034 %, 0.035 %, 0.036 %, 0.037 %, 0.038 %, 0.039 %, 0.04 %, 0.041 %, 0.042 %, 0.043 %, 0.044 %, 0.045 %, 0.046 %, 0.047 %, 0.048 %, 0.049 %, 0.05 %, 0.051 %, 0.052 %, 0.053 %, 0.054 %, 0.055 %, 0.056 %, 0.057 %, 0.058 %, 0.059 %, 0.06 %, 0.061 %, 0.062 %, 0.063 %, 0.064 %, 0.065 %, 0.066 %, 0.067 %, 0.068 %, 0.069 %, 0.07 %, 0.071 %,0.072 %, 0.073 %, 0.074 %, 0.075 %, 0.076 %, 0.077 %, 0.078 %, 0.079 %, 0.08 %, 0.081 %, 0.082 %, 0.083 %, 0.084 %, 0.085 %, 0.086 %, 0.087 %, 0.088 %, 0.089 %, 0.09 %, 0.091 %, 0.092 %, 0.093 %, 0.094 %, 0.095 %,0.096 %, 0.097 %, 0.098 %, 0.099 %, 0.1 %, 0.11 %,0.12 %, 0.13 %, 0.14 %, 0.15 %, 0.16 %, 0.17 %, 0.18 %, 0.19 %, 0.2 %, 0.21 %, 0.22 %, 0.23 %, 0.24 %, or 0.25 % Cr. All expressed in wt. %. In some cases, Cr is not present in the alloy (i.e., 0 %). In some examples, Cr can control grain structure and prevent grain growth and recrystallization. Higher amounts of Cr can provide a higher formability and improved bendability in aged temper.

[0042] In certain examples, the alloy can include manganese (Mn) in an amount up to 0.35 % (e.g., from 0.05 % to 0.18 % or from 0.1 % to 0.35 %) based on the total weight of the alloy. For example, the alloy can include t 0.001 %, 0.002 %, 0.003 %, 0.004 %, 0.005 %, 0.006 %, 0.007 %, 0.008 %, 0.059 %, 0.01 %, 0.011 %, 0.012 %, 0.013 %, 0.014 %, 0.015 %, 0.016 %, 0.017 %, 0.018 %, 0.019 %, 0.02 %, 0.021 %, 0.022 %, 0.023 %, 0.024 %, 0.025 %,0.026 %, 0.027 %, 0.028 %, 0.029 %, 0.03 %, 0.031 %,0.032 %, 0.033 %, 0.034 %, 0.035 %, 0.036 %, 0.037 %, 0.038 %, 0.039 %, 0.04 %, 0.041 %, 0.042 %, 0.043 %, 0.044 %, 0.045 %, 0.046 %, 0.047 %, 0.048 %, 0.049 %,0.05 %, 0.051 %, 0.052 %, 0.053 %, 0.054 %, 0.055 %,0.056 %, 0.057 %, 0.058 %, 0.059 %, 0.06 %, 0.061 %,0.062 %, 0.063 %, 0.064 %, 0.065 %, 0.066 %, 0.067 %,0.068 %, 0.069 %, 0.07 %, 0.071 %, 0.072 %, 0.073 %,0.074 %, 0.075 %, 0.076 %, 0.077 %, 0.078 %, 0.079 %,0.08 %, 0.081 %, 0.082 %, 0.083 %, 0.084 %, 0.085 %,0.086 %, 0.087 %, 0.088 %, 0.089 %, 0.09 %, 0.091 %, 0.092 %, 0.093 %, 0.094 %, 0.095 %, 0.096 %, 0.097 %, 0.098 %, 0.099 %, 0.1 %, 0.11 %, 0.12 %, 0.13 %, 0.14 %, 0.15 %, 0.16 %, 0.17 %, 0.18 %, 0.19 %, 0.2 %, 0.21 %, 0.22 %, 0.23 %, 0.24 %, 0.25 %, 0.26 %, 0.27 %, 0.28 %, 0.29 %, 0.3 %, 0. 31 %, 0.32 %, 0.33 %, 0.34 %, or 0.35% Mn. In some cases, Mn is not present in the alloy (i.e., 0 %). All expressed in wt. %.

[0043] In certain aspects, the alloy also includes iron (Fe) in an amount up to 0.4 % (e.g., from 0.1 % to 0.25 %, from 0.18 % to 0.25 %, from 0.2 % to 0.21 %, or from 0.15 % to 0.32 %) based on the total weight of the alloy. For example, the alloy can include 0.01 %, 0.02 %, 0.03 %, 0.04 %, 0.05 %, 0.06 %, 0.07 %, 0.08 %, 0.09 %, 0.1 %, 0.11 %, 0.12 %, 0.13 %, 0.14 %, 0.15 %, 0.16 %, 0.17 %, 0.18 %, 0.19 %, 0.2 %, 0.21 %, 0.22 %, 0.23 %, 0.24 %, 0.25 %, 0.26 %, 0.27 %, 0.28 %, 0.29 %, 0.3 %, 0.31 %, 0.32 %, 0.33 %, 0.34 %, 0.35 %, 0.36 %, 0.37 %, 0.38 %, 0.39 %, or 0.40 % Fe. In some cases, Fe is not present in the alloy (i.e., 0 %). All expressed in wt. %.

[0044] In certain aspects, the alloy includes zirconium (Zr) in an amount up to 0.25 % (e.g., from 0 % to 0.2 %, from 0.01 % to 0.25 %, from 0.01 % to 0.15 %, from 0.01 % to 0.1 %, or from 0.02 % to 0.09 %) based on the total weight of the alloy. For example, the alloy can include 0.001 %, 0.002 %, 0.003 %, 0.004 %, 0.005 %, 0.006 %, 0.007 %, 0.008 %, 0.009 %, 0.01 %, 0.02 %, 0.03 %, 0.04 %, 0.05 %, 0.06 %, 0.07 %, 0.08 %, 0.09 %, 0.1 %, 0.11 %, 0.12 %, 0.13 %, 0.14 %, 0.15 %, 0.16 %, 0.17 %, 0.18 %, 0.19 %, 0.2 %, 0.21 %, 0.22 %, 0.23 %, 0.24 %, or 0.25 % Zr. In certain aspects, Zr is not present in the alloy (i.e., 0 %). All expressed in wt. %. In some examples, Zr can control grain structure and prevent grain growth and recrystallization. Higher amounts of Zr can provide a higher formability and improved bendability as well in T4 and aged temper.

[0045] In certain aspects, the alloy described herein includes zinc (Zn) in an amount from 0.06 % up to 0.3% (e.g., from 0.06 % to 0.3 %, from 0.06 % to 0.09 %, from 0.06 % to 0.3 %, from 0.06 % to 0.2 %, or from 0.06 % to 0.1 %) based on the total weight of the alloy. For example, the alloy can include 0.06 %, 0.07 %, 0.08 %, 0.09 %, 0.1 %, 0.11 %, 0.12 %, 0.13 %, 0.14 %, 0.15 %, 0.16 %, 0.17 %, 0.18 %, 0.19 %, 0.2 %, 0.21 %, 0.22 %, 0.23 %, 0.24 %, 0.25 %, 0.26 %, 0.27 %, 0.28 %, 0.29 % or 0.3 % Zn. All expressed in wt. %. In certain aspects, Zn can benefit forming, including bending and the reduction of bending anisotropy in plate products.

[0046] In certain aspects, the alloy includes titanium (Ti) in an amount of up to 0.3 % (e.g., from 0.01 % to 0.25 %, from 0.05 % to 0.2 %, or up to 0.1 %) based on the total weight of the alloy. For example, the alloy can include 0.01 %, 0.011 %, 0.012 %, 0.013 %, 0.014 %, 0.015 %, 0.016 %, 0.017 %, 0.018 %, 0.019 %, 0.02 %, 0.025 %, 0.03 %, 0.035 %, 0.04 %, 0.045 %, 0.05 %, 0.055 %,0.06 %, 0.065 %, 0.07 %, 0.075 %, 0.08 %, 0.085 %, 0.09 %, 0.095 %, 0.1 %, 0.11 %, 0.12 %, 0.13 %, 0.14 %, 0.15 %, 0.16 %, 0.17 %, 0.18 %, 0.19 %, 0.2 %, 0.21 %, 0.22 %, 0.23 %, 0.24 %, 0.25 %, 0.26 %, 0.27 %, 0.28 %, 0.29 %, or 0.3 % Ti. All expressed in wt. %.

[0047] In certain aspects, the alloy includes nickel (Ni) in an amount up to 0.04 % (e.g., from 0 % to 0.02 %, from 0.01 % to 0.03 %, from 0.03 % to 0.04 %) based on the total weight of the alloy. For example, the alloy can include 0.001 %, 0.005 %, 0.01 %, 0.011 %, 0.012 %, 0.013 %, 0.014 %, 0.015 %, 0.016 %, 0.017 %, 0.018 %, 0.019 %, 0.02 %, 0.021 %, 0.022 %, 0.023 %, 0.024 %, 0.025 %, 0.026 %, 0.027 %, 0.028 %, 0.029 %, 0.03 %, 0.031 %, 0.032 %, 0.033 %, 0.034 %, 0.035 %, 0.036 %, 0.037 %, 0.038 %, 0.039 %, or 0.04 % %Ni. In certain aspects, Ni is not present in the alloy (i.e., 0 %). All expressed in wt. %.

[0048] Optionally, the alloy compositions can further include other minor elements, sometimes referred to as impurities, in amounts of 0.05 % or below, 0.04 % or below, 0.03 % or below, 0.02 % or below, or 0.01 % or below each. These impurities may include, but are not limited to, V, Ga, Ca, Hf, Sr, Sc, Sn, or combinations thereof. Accordingly, V, Ga, Ca, Hf, Sr, Sc, or Sn may be present in an alloy in amounts of 0.05 % or below, 0.04 % or below, 0.03 % or below, 0.02 % or below, or 0.01 % or below. In certain aspects, the sum of all impurities does not exceed 0.15 % (e.g., 0.1 %). All expressed in wt. %. In certain aspects, the remaining percentage of the alloy is aluminum.

[0049] An exemplary alloy includes 1.11 % Si, 0.72 % Cu, 1.00 % Mg, 0.22 % Fe, 0.3 % Mn, 0.021 % Ti, 0.03 % Cr, 0.2 % Zn, 0.034 % Ni, and up to 0.15 % total impurities, with the remainder Al.

[0050] Another exemplary alloy includes 0.7 % Si, 0.9 % Cu, 0.9 % Mg, 0.22 % Fe, 0.3 % Mn, 0.021 % Ti, 0.03 % Cr, 0.2 % Zn, 0.034 % Ni, and up to 0.15 % total impurities, with the remainder Al.

[0051] Another exemplary alloy includes 0.69 % Si, 0.79 % Cu, 0.9 % Mg, 0.22 % Fe, 0.03 % Mn, 0.023 % Ti, 0.25 % Cr, 0.063 % Zn, 0.0046 % Ni, and up to 0.15 % total impurities (including 0.016 % V), with the remainder Al.

Methods of Making



[0052] In certain aspects, the disclosed alloy composition is a product of a disclosed method. Without intending to limit the disclosure, aluminum alloy properties are partially determined by the formation of microstructures during the alloy's preparation. In certain aspects, the method of preparation for an alloy composition may influence or even determine whether the alloy will have properties adequate for a desired application.

[0053] The alloys described herein can be cast using a casting method as known to those of skill in the art. For example, the casting process can include a Direct Chill (DC) casting process. Optionally, DC cast aluminum alloy products (e.g., ingots) can be scalped before subsequent processing. Optionally, the casting process can include a continuous casting (CC) process. Cast aluminum alloy products can then be subjected to further processing steps. In one non-limiting example, the processing method includes homogenizing, hot rolling, solutionizing, and quenching. In some cases, the processing steps further include annealing and/or cold rolling if desired. In some examples, the processing method also includes a pre-aging step. In some further cases, the processing method can also include a pre-straining step.

Homogenization



[0054] The homogenization step can include heating a cast aluminum alloy product, such as an ingot, prepared from an alloy composition described herein to attain a peak metal temperature (PMT) of, or at least, 520 °C (e.g., at least 520 °C, at least 530 °C, at least 540 °C, at least 550 °C, at least 560 °C, at least 570 °C, or at least 580 °C). The ingot is heated to a temperature of from 520 °C to 580 °C, from 530 °C to 575 °C, from 535 °C to 570 °C, from 540 °C to 565 °C, from 545 °C to 560 °C, from 530 °C to 560 °C, or from 550 °C to 580 °C. In some cases, the heating rate to the PMT can be 100 °C/hour or less, 75 °C/hour or less, 50 °C/hour or less, 40 °C/hour or less, 30 °C/hour or less, 25 °C/hour or less, 20 °C/hour or less, or 15 °C/hour or less. In other cases, the heating rate to the PMT can be from 10 °C/min to 100 °C/min (e.g., 10 °C/min to 90 °C/min, 10 °C/min to 70 °C/min, 10 °C/min to 60 °C/min, from 20 °C/min to 90 °C/min, from 30 °C/min to 80 °C/min, from 40 °C/min to 70 °C/min, or from 50 °C/min to 60 °C/min).

[0055] The cast aluminum alloy product is then allowed to soak (i.e., held at the indicated temperature) for a period of time. The cast aluminum alloy product is allowed to soak for up to 18 hours (from 30 minutes to 18 hours, inclusively). For example, the cast aluminum alloy product can be soaked at a temperature of at least 500 °C for 30 minutes, 1 hour, 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, 10 hours, 11 hours, 12 hours, 13 hours, 14 hours, 15 hours, 16 hours, 17 hours, or 18 hours, or anywhere in between.

Hot Rolling



[0056] Following the homogenization step, a hot rolling step is performed. In certain cases, the cast aluminum alloy products are hot rolled with a hot mill entry temperature of 440 °C - 540 °C. The entry temperature can be, for example, 440 °C, 445 °C, 450 °C, 455 °C, 460 °C, 465 °C, 470 °C, 475 °C, 480 °C, 485 °C, 490 °C, 495 °C, 500 °C, 505 °C, 510 °C, 515 °C, 520 °C, 525 °C, 530 °C, 535 °C, or 540 °C. The hot roll exit temperature ranges from 250 °C -380 °C (e.g., from 330 °C -370 °C). For example, the hot roll exit temperature can be 255 °C, 260 °C, 265 °C, 270 °C, 275 °C, 280 °C, 285 °C, 290 °C, 295 °C, 300 °C, 305 °C, 310 °C, 315 °C, 320 °C, 325 °C, 330 °C, 335 °C, 340 °C, 345 °C, 350 °C, 355 °C, 360 °C, 365 °C, 370 °C, 375 °C, or 380 °C.

[0057] In certain cases, the cast aluminum alloy product can be hot rolled to an 4 mm to 15 mm thick gauge (e.g., from 5 mm to 12 mm thick gauge), which is referred to as a shate. For example, the cast aluminum alloy product can be hot rolled to an 4 mm thick gauge, 5 mm thick gauge, 6 mm thick gauge, 7 mm thick gauge, 8 mm thick gauge, 9 mm thick gauge, 10 mm thick gauge, 11 mm thick gauge, 12 mm thick gauge, 13 mm thick gauge, 14 mm thick gauge, or 15 mm thick gauge. In certain cases, the cast aluminum alloy product can be hot rolled to a gauge greater than 15 mm thick (i.e., a plate). In other cases, the cast aluminum alloy product can be hot rolled to a gauge less than 4 mm (i.e., a sheet). The temper of the as-rolled plates, shates and sheets is referred to as F-temper.

Optional Processing Steps: Annealing Step and Cold Rolling Step



[0058] In certain aspects, the hot-rolled aluminum alloy product undergoes further processing steps after the hot rolling step and before any subsequent steps (e.g., before a solutionizing step). Further processing steps may include an annealing procedure and a cold rolling step.

[0059] The annealing step can result in an aluminum alloy product with improved texture (e.g., an improved T4 alloy) with reduced anisotropy during forming operations, such as stamping, drawing, or bending. By applying the annealing step, the texture in the modified temper is controlled/engineered to be more random and to reduce those texture components (TCs) that can yield strong formability anisotropy (e.g., Goss, Goss-ND, or Cube-RD). This improved texture can potentially reduce the bending anisotropy and can improve the formability in the forming where a drawing or circumferential stamping process is involved, as it acts to reduce the variability in properties at different directions.

[0060] The annealing step can include heating the aluminum alloy product from room temperature to a temperature from 300 °C to 500 °C (e.g., from 305 °C to 495 °C, from 310 °C to 490 °C, from 315 °C to 485 °C, from 320 °C to 480 °C, from 325 °C to 475 °C, from 330 °C to 470 °C, from 335 °C to 465 °C, from 340 °C to 460 °C, from 345 °C to 455 °C, from 350 °C to 450 °C, from 355 °C to 445 °C, from 360 °C to 440 °C, or from 365 °C to 435 °C, from 400 °C to 450 °C, from 425 °C to 475 °C, or from 450 °C to 500 °C).

[0061] The aluminum alloy product can soak at the temperature for a period of time. In one non-limiting example, the alloy is allowed to soak for up to approximately 4 hours (e.g., from 15 to 240 minutes, inclusively). For example, the sheet, plate, or shate can be soaked at the temperature of from 400 °C to 500 °C for 15 minutes, 20 minutes, 25 minutes, 30 minutes, 35 minutes, 40 minutes, 45 minutes, 50 minutes, 55 minutes, 60 minutes, 65 minutes, 70 minutes, 75 minutes, 80 minutes, 85 minutes, 90 minutes, 95 minutes, 100 minutes, 105 minutes, 110 minutes, 115 minutes, 120 minutes, 125 minutes, 130 minutes, 135 minutes, 140 minutes, 145 minutes, 150 minutes, 155 minutes, 160 minutes, 165 minutes, 170 minutes, 175 minutes, 180 minutes, 185 minutes, 190 minutes, 195 minutes, 200 minutes, 205 minutes, 210 minutes, 215 minutes, 220 minutes, 225 minutes, 230 minutes, 235 minutes, or 240 minutes, or anywhere in between. In certain aspects, the aluminum alloy product does not undergo an annealing step.

[0062] A cold rolling step can optionally be applied to the hot-rolled aluminum alloy product before the solutionizing step. In certain aspects, the hot-rolled aluminum alloy product (e.g., the aluminum alloy sheet, plate, or shate) can be cold rolled to a thinner gauge shate or a thinner gauge sheet.

Solutionizing



[0063] The solutionizing step includes heating an aluminum alloy sheet, plate, or shate from room temperature to a temperature of from 520 °C to 580 °C (e.g., from 525 °C to 575 °C, from 530 °C to 570 °C, from 535 °C to 565 °C, from 540 °C to 560 °C, or from 545 °C to 555 °C). The aluminum alloy sheet, plate, or shate can soak at the temperature for a period of time. In certain aspects, the aluminum alloy sheet, plate, or shate is allowed to soak for up to 2 hours (e.g., from 5 seconds to 120 minutes inclusively). For example, the aluminum alloy sheet, plate, or shate can be soaked at the temperature of from 525 °C to 580 °C for 5 seconds, 10 seconds, 15 seconds, 20 seconds, 25 seconds, 30 seconds, 35 seconds, 40 seconds, 45 seconds, 50 seconds, 55 seconds, 60 seconds, 65 seconds, 70 seconds, 75 seconds, 80 seconds, 85 seconds, 90 seconds, 95 seconds, 100 seconds, 105 seconds, 110 seconds, 115 seconds, 120 seconds, 125 seconds, 130 seconds, 135 seconds, 140 seconds, 145 seconds, 150 seconds, 5 minutes, 10 minutes, 15 minutes, 20 minutes, 25 minutes, 30 minutes, 35 minutes, 40 minutes, 45 minutes, 50 minutes, 55 minutes, 60 minutes, 65 minutes, 70 minutes, 75 minutes, 80 minutes, 85 minutes, 90 minutes, 95 minutes, 100 minutes, 105 minutes, 110 minutes, 115 minutes, or 120 minutes, or anywhere in between.

[0064] In certain aspects, the heat treatment is performed immediately after the hot or cold rolling step. In certain aspects, the heat treatment is performed after an annealing step.

Quenching



[0065] In certain aspects, the aluminum alloy sheet, plate, or shate can then be cooled to a temperature of 25 °C to 65 °C at a quench speed that can vary between 50 °C/s to 400 °C/s in a quenching step that is based on the selected gauge. For example, the quench rate can be from 50 °C/s to 375 °C/s, from 60 °C/s to 375 °C/s, from 70 °C/s to 350 °C/s, from 80 °C/s to 325 °C/s, from 90 °C/s to 300 °C/s, from 100 °C/s to 275 °C/s, from 125 °C/s to 250 °C/s, from 150 °C/s to 225 °C/s, or from 175 °C/s to 200 °C/s.

[0066] In the quenching step, the aluminum alloy sheet, plate, or shate is rapidly quenched with a liquid (e.g., water) and/or gas or another selected quench medium. In certain aspects, the aluminum alloy sheet, plate, or shate can be rapidly quenched with water. In certain aspects, the aluminum alloy sheet, plate, or shate can be quenched with air.

Pre-Aging, Pre-Straining, and/or Aging



[0067] A pre-aging step and optionally a pre-straining step, and/or an aging step can be performed prior to downstream thermal treatment processes (e.g., post-forming heat treatment). In some examples, a pre-aging step and an aging step can be performed. In other examples, a pre-aging step and a pre-straining step can be performed. In still other examples, a pre-aging step, a pre-straining step, and an aging step can be performed. In some cases, a pre-straining step and an aging step can be performed.

[0068] The pre-aging step includes heating the aluminum alloy sheet, plate, or shate after the solutionizing step to a temperature of from 115 °C to 135 °C (e.g., 120 °C to 135 °C, 125 °C to 135 °C). The pre-aging step includes heating the aluminum alloy sheet, plate, or shate after solutionizing from 115 °C to 135 °C (e.g., from 120 °C to 130 °C). The aluminum alloy sheet, plate, or shate can soak at the temperature for a period of time. In certain aspects, the aluminum alloy sheet, plate, or shate is allowed to soak for up to 2 hours (e.g., for up to 10 minutes, for up to 20 minutes, for up to 30 minutes, for up to 40 minutes, for up to 45 minutes, for up to 60 minutes, for up to 90 minutes). The time between solutionizing and pre-aging can be between 0 minutes and 60 minutes. For example, the time between solutionizing and pre-aging can be between 5 minutes and 45 minutes or between 10 minutes and 35 minutes. In some examples, pre-aging can inhibit natural age hardening of aluminum alloys. In some further examples, the pre-aging step can be combined with one or more downstream thermal treatment processes. Such a combination of the pre-aging step and downstream thermal treatment step(s) can provide an aluminum alloy product with high strength and high deformability (e.g., formability, bendability, crushability, or crashability).

[0069] The methods can optionally include a pre-straining step. The pre-straining step can include partially deforming the aluminum alloy sheet, plate, or shate in a direction longitudinal to a rolling direction. For example, the pre-straining step can include applying a tensile strain to the aluminum alloy sheet, plate, or shate providing up to 10 % elongation. For example, the elongation can be up to 1 %, up to 2 %, up to 3 %, up to 4 %, up to 5 %, up to 6 %, up to 7 %, up to 8 %, up to 9 %, or up to 10 %. In some further examples, the pre-straining step can be combined with one or more downstream thermal treatment processes. Such a combination of the pre-straining step and downstream thermal treatment processes can provide an aluminum alloy product with high strength and high deformability (e.g., formability, bendability, crushability, or crashability).

[0070] Optionally, the methods can further include an aging step. Optionally, the alloy can be naturally aged for a period of time to result in the T4 temper. In certain aspects, the alloy in the T4 temper can be artificially aged at 160 °C to 225 °C (e.g., 165 °C, 170 °C, 175 °C, 180 °C, 185 °C, 190 °C, 195 °C, 200 °C, 205 °C, 210 °C, 215 °C, 220 °C, or 225 °C) for a period of time. Optionally, the alloy can be artificially aged for a period from 5 minutes to 10 hours (e.g., 5 minutes, 10 minutes, 15 minutes, 30 minutes, 1 hour, 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, or 10 hours, or anywhere in between) to result in an exemplary temper. In some aspects, pre-aging the alloy after solutionizing the alloy to result in the exemplary temper can prevent further natural aging from occurring. Non-natural aging can provide constant material properties over time (e.g., yield strength and bendability do not degrade over time) and can reduce the difference of mechanical properties when subjecting the alloy to a downstream processing step (e.g., cold forming and/or stamping.).

Coiling



[0071] The aluminum alloy sheet, plate, or shate can be gathered at a terminal point of a production line to form an aluminum alloy coil.

Alloy Properties


Effect of pre-aging on alloy properties



[0072] In some non-limiting examples, the alloys described herein can have high strength and high formability and bendability when subjected to pre-aging after solutionizing, as compared to conventional heat treatable alloys not processed according to the methods described herein. In certain cases, the alloys also demonstrate a resistance to age hardening after solutionizing. In further examples, the alloys exhibit stable strength and formability after solutionizing.

[0073] In certain aspects, the aluminum alloys may have an in-service strength (e.g., strength of an aluminum alloy employed on a vehicle) of at least 150 MPa. In non-limiting examples, the in-service strength is at least 180 MPa, at least 190 MPa, at least 195 MPa, at least 200 MPa, at least 210 MPa, at least 220 MPa, at least 230 MPa, at least 240 MPa, at least 250 MPa, at least 260 MPa, at least 270 MPa, at least 280 MPa, at least 290 MPa, at least 295 MPa, at least 300 MPa, at least 305 MPa, at least 310 MPa, at least 315 MPa, at least 320 MPa, at least 325 MPa, at least 330 MPa, at least 335 MPa, at least 340 MPa, at least 345 MPa, at least 350 MPa, at least 355 MPa, or at least 360 MPa. In some cases, the in-service strength is from 240 MPa to 340 MPa. For example, the in-service strength can be from 150 MPa to 295 MPa, from 175 MPa to 275 MPa, from 200 MPa to 250 MPa, from 180 MPa to 190 MPa, or from 185 MPa to 195 MPa.

[0074] In certain aspects, the alloys exhibit a uniform elongation of greater than or equal to 19 % and a total elongation of greater than or equal to 25 %. In certain aspects, the alloys exhibit a uniform elongation of greater than or equal to 22 % and a total elongation of greater than or equal to 27 %. For example, the alloys can exhibit a uniform elongation of 19 % or more, 20 % or more, 21 % or more, 22 % or more, 23 % or more, 24 % or more, 25 % or more, 26 % or more, 27 % or more, or 28 % or more. The alloys can exhibit a total elongation of 25 % or more, 26 % or more, 27 % or more, 28 % or more, 29 % or more, or 30 % or more.

[0075] The mechanical properties of the aluminum alloys can be controlled by various processing conditions depending on the desired use. As one example, the alloys can be produced (or provided) in the T3 temper, the T4 temper, the T6 temper or the T8 temper. In some non-limiting examples, T4 sheets, plates, and shates can be subjected to additional processing treatment(s) to meet strength requirements upon receipt and further processing by an end user. In some cases, the alloy can be provided in a T4 temper after being subjected to a pre-aging step, wherein the pre-aging step enables the alloy to achieve T6 temper properties after an end user's paint bake procedure. For example, sheets, plates, and shates can be delivered in T4 temper, coated via Zn-phosphating and electro-coating (E-coating) by an end user, and thermally treated (e.g., paint baked) to cure the coating. Paint baking a pre-aged aluminum alloy can complete an artificial aging process providing an aluminum alloy product exhibiting mechanical properties of an aluminum alloy product delivered in a T6 temper. Surprisingly, combining pre-aging with paint baking provides high strength, comparable to levels observed in T6 temper aluminum alloys, and high deformability, comparable to levels observed in T4 temper aluminum alloys.

Effect of pre-straining on alloy properties



[0076] In some cases, the alloys can be provided in a T3 temper after being subjected to a pre-straining step. In some non-limiting examples, T3 sheets, plates, and shates can be subjected to additional processing treatment(s) to meet strength requirements upon receipt and further processing by an end user. In some cases, the alloys can be provided in a T3 temper after being subjected to a pre-straining step. The pre-straining step enables the alloys to achieve T6 temper properties after an end user's forming and post-forming heat treatment (PFHT) procedures. For example, sheets, plates, and shates can be delivered in T3 temper, formed into an aluminum alloy part by an end user, and thermally treated (e.g., by applying a PFHT). Applying a PFHT to a pre-strained aluminum alloy can complete an artificial aging process providing an aluminum alloy product exhibiting the mechanical properties of an aluminum alloy product delivered in a T6 temper. Surprisingly, combining pre-straining with PFHT provides high strength, comparable to levels observed in T6 temper aluminum alloys, and high deformability, comparable to levels observed in T4 temper aluminum alloys. In certain aspects, the pre-strained alloys exhibit a uniform elongation of 12 % or greater (e.g., greater than 15 % or greater than 20 %) for a 10 % prestrain.

Methods of Using



[0077] The alloys and methods described herein can be used in automotive, electronics, and transportation applications, such as commercial vehicle, aircraft, or railway applications. For example, the aluminum alloy products described herein could be used for chassis, crossmember, and intra-chassis components (encompassing, but not limited to, all components between the two C channels in a commercial vehicle chassis) to gain strength, serving as a full or partial replacement of high-strength steels. In certain aspects, the aluminum alloy products are useful in applications where the processing and operating temperature is approximately 100 °C or lower.

[0078] In certain aspects, the alloys and methods can be used to prepare motor vehicle body part products. For example, the disclosed alloys and methods can be used to prepare automobile body parts, such as bumpers, side beams, roof beams, cross beams, pillar reinforcements (e.g., A-pillars, B-pillars, and C-pillars), inner panels, side panels, floor panels, tunnels, structure panels, reinforcement panels, inner hoods, or trunk lid panels. The disclosed aluminum alloys and methods can also be used in aircraft or railway vehicle applications, to prepare, for example, external and internal panels. In certain aspects, the disclosed alloys can be used for other specialties applications, such as automotive battery plates/shates.

[0079] In certain aspects, the products created from the alloys and methods can be coated. For example, the disclosed products can be Zn-phosphated and electrocoated (E-coated). As part of the coating procedure, the coated samples can be baked to dry the E-coat at 160 °C to 205 °C for 10 minutes to 30 minutes (e.g., 170 °C for 25 minutes, 200 °C for 15 minutes, or 180 °C for 20 minutes). In certain aspects, a paint bake response is observed wherein the alloys exhibit an increase in yield strength. In certain examples, the paint bake response is employed to complete an artificial aging process initiated by a pre-aging step employed during aluminum alloy production.

[0080] In certain aspects, the products created from the alloys and methods can be formed. For example, the disclosed products can be drawn or circumferentially stamped. As part of the forming procedure, the formed samples can be baked to anneal the formed aluminum alloy part at 160 °C to 225 °C for 15 minutes to 45 minutes (e.g., 180 °C for 35 minutes, 215 °C for 25 minutes, or 195 °C for 30 minutes). In certain aspects, an artificial aging response is observed wherein the alloys exhibit an increase in yield strength. Surprisingly, the alloys do not exhibit a loss of deformability normally observed in artificially aged aluminum alloys. The alloys and methods described herein provide high strength alloys that are also highly deformable.

[0081] The described alloys and methods can also be used to prepare housings for electronic devices, including mobile phones and tablet computers. For example, the alloys can be used to prepare housings for the outer casing of mobile phones (e.g., smart phones) and tablet bottom chassis, with or without anodizing. Exemplary consumer electronic products include mobile phones, audio devices, video devices, cameras, laptop computers, desktop computers, tablet computers, televisions, displays, household appliances, video playback and recording devices, and the like. Exemplary consumer electronic product parts include outer housings (e.g., facades) and inner pieces for the consumer electronic products.

[0082] In certain examples, the alloys can be used in an exemplary temper as described herein. In certain aspects, the alloys and methods described herein results in a high-strength alloy including formability properties normally observed in lower strength alloys. Additionally, the resulting exemplary temper can provide alloys that do not naturally age-harden over time. A non-natural aging alloy can be stored indefinitely and retain desirable mechanical properties including high-strength, high formability and a favorable paint bake response.

[0083] The following examples will serve to further illustrate the present invention without, however, constituting any limitation thereof. On the contrary, it is to be clearly understood that resort may be had to various embodiments, modifications and equivalents thereof which, after reading the description herein, may suggest themselves to those skilled in the art without departing from the spirit of the invention. During the studies described in the following examples, conventional procedures were followed, unless otherwise stated. Some of the procedures are described below for illustrative purposes.

EXAMPLES


Example 1: Effect of pre-aging after solutionizing on natural aging



[0084] An exemplary 6xxx series aluminum alloy was produced according to the methods described herein. Addition of a pre-aging step after the solutionizing step provided an aluminum alloy in a pre-aged condition resulting in an exemplary temper. Normally, 6xxx alloys age-harden over time when stored at room temperature. This age-hardening is demonstrated by a logarithmic increase in tensile strength (Rp02) over time (see Figure 1 "no PX," referring to no pre-aging). Pre-aging the alloy after solutionizing the alloy can pre-age the alloy before artificial or natural aging can be employed in optional downstream processing. With this exemplary pre-aging, the alloy stays at the same Rp02 level when stored for a period of time at room temperature. Figure 1 compares the effect of the pre-aging at two different temperatures to a sample that was not pre-aged. The top curve corresponds to pre-aging at 120 °C for 2 hours (this curve is also typical of alloys subjected to coil cooling from 130 °C); the middle curve corresponds to pre-aging at 100 °C for 2 hours (this curve is also typical of alloys subjected to coil cooling from 110 °C); and the bottom curve corresponds to samples that were not subjected to a pre-aging step (this curve is also typical of alloys subjected to coil cooling from less than 50 °C), referred to as "no PX."

[0085] A pre-aged alloy resistant to natural age-hardening can exhibit an increased shelf life (e.g., for up to greater than 1 year) for storing as-produced aluminum alloys. In order to demonstrate the effect of the exemplary temper on the mechanical properties, the exemplary alloy with the composition described in Table 4 above was produced with different pre-aging temperatures. The various temperatures were recorded at the exit of the pre-aging furnace: 50 °C (no PX), 110 °C (100 °C / 2 hours) and 130 °C (120 °C / 2 hours). The exemplary alloy pre-aged at 120 °C demonstrated a higher yield strength than those pre-aged at 100 °C and not pre-aged, and the yield strength remained stable over a period of time.

Example 2: Effect of pre-aging after solutionizing on formability



[0086] An exemplary alloy with the composition described in Table 4 was produced with different pre-aging temperatures as described in Example 1. Figure 2 shows the stability of the elongation (Ag) over time for the exemplary alloy in the exemplary temper. The elongation is highly stable and does not decrease as strength increases.

Example 3: Effect of pre-aging after solutionizing on paint bake response



[0087] An exemplary alloy with the composition described in Table 4 was produced with different pre-aging temperatures as described in Example 1. Figure 3 shows the effect of the pre-aging after solutionizing of an aluminum alloy on an optional downstream process wherein a coated aluminum alloy is heated to cure the coating. Coat curing, or paint baking, is known to a person of ordinary skill in the art to further artificially age an aluminum alloy and further increase the yield strength of the alloy. An exemplary alloy sample was subjected to a paint bake of 185 °C for 20 minutes after solutionizing and after pre-straining by 2%. Figure 3 demonstrates the increased yield strength after paint baking of the exemplary alloy in the exemplary temper (center group of histograms) compared to the yield strength after paint baking of the exemplary alloy in T4 temper (left group of histograms). The right group of histograms referred to as "Paint Bake" indicates the difference in the paint bake response of the alloys in the exemplary temper over the alloys in T4 temper. The left histogram bar in each group corresponds to the sample that was not pre-aged ("no PX"); the center histogram bar in each group corresponds to the sample pre-aged at conditions of 100 °C / 2 hours; and the right histogram bar in each group corresponds to the sample pre-aged at conditions of 120 °C / 2 hours. This example shows that a very high paint bake response can be achieved with the exemplary alloys. The exemplary alloys demonstrated yield strength greater than 300 MPa when pre-aged at 120 °C for 2 hours after solutionizing, pre-straining by 2% and paint baking at 185 °C for 20 minutes.

Example 4: Effect of pre-aging temperature on mechanical properties



[0088] As described above, three different pre-aging conditions were considered. Coil cooling rates were recorded upon exit from a continuous heat treatment line. Coil cooling curves are presented in Figure 4. A non-pre-aged coil cools to room temperature faster than the pre-aged coils (bottom curve, no PX). The cooling rate curves for the pre-aged coils show a higher initial cooling rate for the coil pre-aged at a higher temperature (top curve, 120 °C / 2 hours). The middle curve shows the cooling rate for the coil pre-aged at 100 °C / 2 hours. The cooling rates for the pre-aged coils eventually equilibrate allowing the pre-aged coils to arrive at similar temperatures after similar periods of time.

[0089] A comparative alloy, AA6014, was subjected to the methods described herein resulting in the exemplary temper and naturally aged resulting in T4 temper. Figure 5 presents the temperature data recorded on the coil at three different positions upon exit from the heat treatment line. Over time, the temperature of the coil equilibrated resulting in roughly the same temperature across the entirety of the coil, about 125 °C. Figure 6 shows the stability of the yield strength of the comparative AA6014 aluminum alloy in T4 temper over time of samples taken from the three different positions. The varied yield strengths of the different samples exhibits a non-uniform aging within the coil. Figure 7 presents the yield strength data from the comparative AA6014 alloy subjected to the pre-aging step resulting in the exemplary temper. The recorded yield strengths are similar for each of the samples taken from different positions suggesting a uniform aluminum alloy coil. Additionally, there is no evidence of natural aging after solutionizing demonstrating the effect of the exemplary temper. Figure 8 presents the elongation (Ag) data from the comparative AA6014 alloy subjected to the pre-aging step resulting in the exemplary temper. The elongation data suggest uniform formability as well as resistance to natural aging of the alloy in the exemplary temper.

[0090] A second comparative alloy, AA6111, was subjected to pre-aging to result in the exemplary temper. The comparative AA6111 was pre-aged at 100 °C for 2 hours after solutionizing. After solutionizing, the comparative AA6111 alloy was stored at room temperature and yield strength was tested periodically. Figure 9 presents the yield strength stability of the comparative AA6111 in exemplary temper. The effects of natural aging are evident in the graph as a 30 - 40 MPa increase in yield strength was observed over a period of about 5 months. The comparative AA6111 alloy in the exemplary temper was pre-aged at 120 °C for 2 hours (or coil cooled from 130 °C) after solutionizing and stored at room temperature. Yield strength was tested periodically. Figure 10 shows the results of the strength tests, indicating a very slight increase in yield strength (about 2 MPa) over a period of about 6 months, demonstrating the resistance to natural aging of the comparative AA6111 alloy in the exemplary temper, showing the desired properties of the exemplary temper can be composition specific (i.e., the exemplary temper does not show resistance to natural aging in all 6xxx series aluminum alloys).

Example 5: Process optimization



[0091] A variety of pre-aging temperatures were evaluated for optimal resulting properties. Figure 11 shows the effect on the in service yield strength after 2% pre-strain and temperature aging of 185 °C for 20 minutes for a range of pre-aging temperatures on the paint bake. Higher pre-aging temperatures resulted in very high yield strength after solutionizing and paint baking. Figure 12 shows the paint bake response as a function of: the difference in the paint bake response of the alloys in the exemplary temper as compared to the alloys in T4 temper (referred to as "BH" in Figure 12); versus various pre-aging temperatures and various natural aging (e.g., 1 week, 1 month, 3 months, and 6 months). For an exemplary alloy as described herein (see Table 4), an optimum pre-aging temperature for maximum bake hardening is 100 °C/2 hours (or coil cooling from 110 °C). However, to provide stable mechanical properties over time, the optimum pre-aging temperature is from about 110 °C to about 120 °C for 2 hours (which is similar to coil cooling from about 120 to about 130 °C, a typical exit temperature from a pre-aging furnace on a continuous heat treatment line). Further optimization included a formability study. Figure 13 presents the paint bake response as a function of the strain hardening exponent (n-value) in T4 temper. A higher n-value indicates higher formability in T4 temper. An n-value of at least 0.23 is required for 6xxx series aluminum alloys in T4 temper and is desired for aluminum alloys in the exemplary temper to have desired formability. The graph indicates the optimal pre-aging temperature is from about 115 °C to about 135 °C, preferably from 120 °C to 130 °C.

[0092] The exemplary alloy (see Table 4) was stored at room temperature to assess natural aging effects observed for the exemplary alloy pre-aged at various temperatures. Figure 14 presents the results from one week of natural aging, one month of natural aging, three months of natural aging, and six months of natural aging. Evident in the graph, a greater pre-aging temperature can provide a decreased natural aging effect. Figure 15 presents the difference of the alloy yield strength (Rp02) measured after one week (7 days) and the alloy yield strength measured after one month (31 days). Higher pre-aging temperatures prevent natural aging effects as evident in the figure. The alloy strength did not increase after one month of natural aging when the pre-aging temperature was greater than 120 °C. An optimum pre-aging temperature was determined to be greater than 110 °C, where the change in alloy yield strength (Rp02) is less than 2 MPa. Additionally, a higher pre-aging temperature did not deteriorate the bendability of the exemplary alloys in T6 temper (accomplished by artificially aging at 180 °C for 10 hours). Figure 16 shows no difference in the alloy bendability when subjected to pre-aging over a range of temperatures from 90 °C to 160 °C. Figure 17 presents the n-values plotted over time for various samples subjected to natural aging. Higher n-values are desired for forming difficult metal structures. Very good n-values were demonstrated by alloy samples pre-aged at temperatures less than 140 °C. Additionally, when subjected to pre-aging at temperatures ranging from 110 °C to 130 °C, the exemplary alloy exhibited no decrease of the n-value for a time period of at least 6 months. The stable n-value indicates stable forming properties. In comparison, when subjected to pre-aging at temperatures less than 110 °C, the exemplary alloy exhibited a decrease of the n-value over 6 months. An unstable n-value can indicate stable forming can only be performed at an optimum time before stability of the forming properties can degrade.

[0093] Optimum pre-aging was determined by maximizing the paint bake response, stabilizing strength and elongation over time and maximizing the alloy bendability.

Example 6: Comparing an exemplary alloy and comparative alloy AA6014



[0094] An exemplary alloy as described herein (see Table 4) is compared to an AA6014 aluminum alloy. Both alloys were pre-aged after solutionizing at 130 °C upon exit from a continuous heat treatment line. Figure 18 shows elongation (Ag) measured at different time intervals after solution heat treatment (SHT). Both alloys show very stable elongation over time, and the exemplary alloy demonstrates much higher elongation than the comparative AA6014 alloy. As noted above, the pre-aging process can be composition dependent.

Example 7: Effect of pre-aging on comparative alloys



[0095] Three comparative alloys were pre-aged after laboratory solution heat treatment at various temperatures and stored at room temperature to evaluate the natural aging effect on the comparative alloys. The comparative alloys included a high strength AA6016 aluminum alloy (referred to as "AA6016-HS"), a highly formable AA6016 aluminum alloy (referred to as "AA6016-HF"), and an AA6014 aluminum alloy. The chemical compositions of the comparative alloys are listed in Table 5 below:
Table 5
AlloyAA6016-HSAA6016-HFAA6014
ElementWeight Percentage (wt. %)Weight Percentage (wt. %)Weight Percentage (wt. %)
Cu 0.038 0.109 0.096
Si 1.04 1.26 0.55
Mg 0.51 0.273 0.59
Cr 0.0049 0.0078 0.0058
Mn 0.079 0.059 0.047
Fe 0.176 0.146 0.158
Zr 0.001 0.001 0.001
Zn 0.057 0.0068 0.0085
Ti 0.0199 0.0212 0.014
Ni 0.0043 0.0027 0.0044
Impurities 0.0 - 0.05 (each)
0.0 - 0.15 (total)
Al Remainder


[0096] Figure 19 is a graph showing the effect of pre-aging temperature on comparative alloy AA6016-HS (see Table 5). Pre-aging temperatures were evaluated in a range from about room temperature to 160 °C. Pre-aging was performed for 2 hours at temperatures of 25 °C, 90 °C, 100 °C, 110 °C, 120 °C, 130 °C, 140 °C, and 160 °C. After pre-aging, the comparative alloys were subjected to natural aging (referred to as "T4" in Figure 19), artificial aging for 10 hours at a temperature of 180 °C (referred to as "T6" in Figure 19), and paint baking for 20 minutes at a temperature of 185 °C after 2% pre-straining (referred to as "T8x" in Figure 19). Evident in the graph, natural aging effects decrease when the comparative alloys samples were pre-aged at a temperature of at least 130 °C. The comparative alloy subjected to artificial aging for 10 hours at a temperature of 180 °C (T6) and paint baking for 20 minutes at a temperature of 185 °C after 2% pre-straining (T8x) exhibited a maximum yield strength of about 280 MPa.

[0097] Figure 20 is a graph showing the effect of pre-aging temperature on comparative alloy AA6016-HF (see Table 5). Pre-aging temperatures were evaluated in a range from about room temperature to 160 °C. Pre-aging was performed for 2 hours at temperatures of 25 °C, 90 °C, 100 °C, 110 °C, 120 °C, 130 °C, 140 °C, and 160 °C. After pre-aging, the comparative alloys were subjected to natural aging (referred to as "T4" in Figure 20), artificial aging for 10 hours at a temperature of 180 °C (referred to as "T6" in Figure 20), and paint baking for 20 minutes at a temperature of 185 °C after 2% pre-straining (referred to as "T8x" in Figure 20). Evident in the graph, natural aging effects decrease when the comparative alloys samples were pre-aged at a temperature of at least 130 °C. The comparative alloy subjected to artificial aging for 10 hours at a temperature of 180 °C (T6) exhibited a maximum yield strength of about 250 MPa. The comparative alloy subjected to paint baking for 20 minutes at a temperature of 185 °C after 2% pre-straining (T8x) exhibited a maximum yield strength of about 220 MPa.

[0098] Figure 21 is a graph showing the effect of pre-aging temperature on comparative alloy AA6014 (see Table 5). Pre-aging temperatures were evaluated in a range from about room temperature to 160 °C. Pre-aging was performed for 2 hours at temperatures of 25 °C, 90 °C, 100 °C, 110 °C, 120 °C, 130 °C, 140 °C, and 160 °C. After pre-aging, the comparative alloys were subjected to natural aging (referred to as "T4" in Figure 21), artificial aging for 10 hours at a temperature of 180 °C (referred to as "T6" in Figure 21), and paint baking for 20 minutes at a temperature of 185 °C after 2% pre-straining (referred to as "T8x" in Figure 21). Evident in the graph, natural aging effects decrease when the comparative alloys samples were pre-aged at a temperature of at least 140 °C. The comparative alloy subjected to artificial aging for 10 hours at a temperature of 180 °C (T6) and paint baking for 20 minutes at a temperature of 185 °C after 2% pre-straining (T8x) exhibited a maximum yield strength of about 280 MPa.

[0099] Figures 22A - 22D are graphs showing effects of paint baking on the comparative aluminum alloys in Table 5. Figure 22A shows the effects of paint baking on Alloy AA6016-HS. Figure 22B shows the effect of paint baking on Alloy AA6016-HF. Figure 22C shows the effect of paint baking on Alloy AA6014. Figure 22D shows the effect of paint baking on the exemplary aluminum alloy in Table 3. An increase in strength after paint baking is referred to as "bake hardening," and is calculated by subtracting a measured yield strength of the aluminum alloy not subjected to paint baking from a measured yield strength of the aluminum alloy after paint baking (e.g., paint baking for 20 minutes at a temperature of 185 °C after 2% pre-straining (T8x)). Bake hardening was evaluated for samples stored after paint baking for time periods of 1 week (indicated by solid squares), 1 month (indicated by solid circles), and 3 months (indicated by solid triangles). The exemplary aluminum alloy in Table 3 (Figure 22D) exhibited a greater bake hardening response than the comparative aluminum alloys listed in Table 5 (Figures 22A, 22B, and 22C).

[0100] Figure 23 is a graph showing effects of natural aging on yield strength of the comparative aluminum alloys in Table 5 and of the exemplary aluminum alloy in Table 3. Pre-aging temperatures were evaluated in a range from about room temperature to 160 °C. Pre-aging was performed for 2 hours at temperatures of 25 °C, 90 °C, 100 °C, 110 °C, 120 °C, 130 °C, 140 °C, and 160 °C. After pre-aging, all samples were subjected to natural aging for a time period of 6 months. Evident in the graph of Figure 23, the exemplary aluminum alloy (see Table 3) consistently exhibited the greatest strength.

[0101] Figure 24 is a graph showing effects of natural aging on formability of the comparative aluminum alloys in Table 5 and the exemplary aluminum alloy in Table 3. Pre-aging temperatures were evaluated in a range from about room temperature to 160 °C. Pre-aging was performed for 2 hours at temperatures of 25 °C, 90 °C, 100 °C, 110 °C, 120 °C, 130 °C, 140 °C, and 160 °C. After pre-aging, all samples were subjected to natural aging for a time period of 6 months. Evident in the graph of Figure 24, the exemplary aluminum alloy (see Table 3) exhibited greater n-values when pre-aged at temperatures of at least 110 °C, indicating the exemplary aluminum alloy is more amenable to forming.

[0102] Figure 25 is a graph showing effects of paint baking on yield strength of the comparative aluminum alloys in Table 5 and the exemplary aluminum alloy in Table 3. Pre-aging temperatures were evaluated in a range from about room temperature to 160 °C. Pre-aging was performed for 2 hours at temperatures of 25 °C, 90 °C, 100 °C, 110 °C, 120 °C, 130 °C, 140 °C, and 160 °C. After pre-aging, all samples were subjected to paint baking for 20 minutes at a temperature of 185 °C after 2% pre-straining (T8x) and subsequently stored for a time period of 6 months. Evident in the graph of Figure 25, the exemplary aluminum alloy (see Table 3) consistently exhibited the greatest strength.

[0103] The exemplary alloy according to Table 3 exhibited very stable forming properties for at least 6 months after solution heat treating, very high n-values after 6 months, and a very high paint bake response for the exemplary alloy in the T8x temper (e.g., after paint baking for 20 minutes at a temperature of 185 °C after 2% pre-straining). Such characteristics indicate a high-strength aluminum alloy amenable to complex forming procedures to provide, for example, automotive B-pillars, structural tunnels, or any suitable complex aluminum alloy article.

[0104] Figure 26A is a graph showing the effect of natural aging on 6 aluminum alloy samples prepared from the exemplary alloy of Table 4. The aluminum alloy samples were subjected to pre-aging at a temperature of 130 °C for 2 hours. The yield strength of each sample was evaluated after about 10 to about 20 days of natural aging, after about 90 to about 100 days of natural aging, and after about 180 to about 190 days of natural aging. Evident in the graph of Figure 26A, any effect of natural aging was insignificant.

[0105] Figure 26B is a graph showing the effect of natural aging on 6 aluminum alloy samples taken from the exemplary alloy as in the example of Table 4. The aluminum alloy samples were subjected to pre-aging at a temperature of 130 °C for 2 hours and subsequently subjected to paint baking for 20 minutes at a temperature of 185 °C after 2% pre-straining (T8x). The yield strength of each sample was evaluated after about 10 to about 20 days of natural aging, after about 90 to about 100 days of natural aging, and after about 180 to about 190 days of natural aging. Evident in the graph of Figure 26B, any effect of natural aging is insignificant and high strength (e.g., greater than about 300 MPa) is maintained after paint baking and at least 6 months of storing.

Example 8: Effect of pre-straining and post-forming heat treatment



[0106] An exemplary thermal process 100 is presented in Figure 27. A heat treatable alloy is subjected to a solutionizing step to evenly distribute alloying elements throughout the aluminum matrix. The solutionizing step can include heating 110 the alloy to above a solutionizing temperature 115 sufficient to soften the aluminum without melting and then maintaining the alloy above the solutionizing temperature 115. The solutionizing step can be performed for a period of time of about 1 minute to about 5 minutes (Range A). Solutionizing can allow the alloying elements to diffuse throughout and distribute evenly within the alloy. Once solutionized, the aluminum alloy is rapidly cooled (i.e., quenched) 120 to freeze the alloying elements in place and prevent the alloying elements from agglomerating and precipitating out of the aluminum matrix.

[0107] The solutionized and quenched exemplary alloy is then subjected to an aging procedure after the quenching step. In some examples the aging step is performed for a period of about 1 minute to about 20 minutes (Range B) after the quenching step. The aging procedure can include a pre-aging step, which includes heating the solutionized and quenched aluminum alloy 130 and cooling 140 for a time period that can be greater than 24 hours (Range C).

[0108] In some cases, an exemplary pre-straining step 150 can be performed in which a uniaxial tension is applied to the alloy providing a plastic elongation of up to 10 %.

[0109] Range E (see Figure 27) can include natural aging 160, coating, forming, or any combination thereof. In some non-limiting examples, natural aging 160 can occur during aluminum alloy storage. In some examples, the aluminum alloy can be coated. In some further examples, the aluminum alloy can be formed into an aluminum alloy part. In some still further examples, the aluminum alloy can be thermally treated (Range F / Range G) after coating or forming. In some cases, the thermal treatment performed after coating, forming, or any combination thereof, can further age harden the aluminum alloy. In some examples, as part of the coating procedure, the coated samples can be heated 170 to about 180 °C, maintained at 180 °C for about 20 minutes 175 and cooled 180 (Range F). As part of the forming procedure, the formed samples can be can be heated 185 to about 195 °C, maintained at 195 °C for about 30 minutes 175 and cooled 195 (Range G).

Example 9: Effect of pre-straining and post-forming heat treatment



[0110] The effects of pre-straining and post-forming on an exemplary aluminum alloy having a composition as described herein were determined. The exemplary alloy used for the tests has the following composition: 0.69 % Si, 0.79 % Cu, 0.9 % Mg, 0.22 % Fe, 0.03 % Mn, 0.023 % Ti, 0.25 % Cr, 0.063 % Zn, 0.0046 % Ni, and 0.016 % V, with the remainder Al.

[0111] Figures 28 and 29 show the changes in deformability and yield strength after various pre-straining and PFHT performed at various temperatures for 30 minutes. Aluminum alloy samples subjected to pre-straining without PFHT are indicated by solid symbols. Aluminum alloy samples subjected to pre-straining with PFHT are indicated by open symbols and connecting lines. PFHT temperature are indicated numerically as provided in Table 6.
Table 6
IndicatorTemperature (°C)
1 160
2 180
3 195
4 205
5 215
6 225


[0112] Figure 28 shows an increase in yield strength (referred to as "Rp") with increasing pre-straining. Figure 28 also shows a decrease in bend angle (referred to as "DC alpha 2.5 mm") with increasing pre-straining. Surprisingly, applying a PFHT step provided increased strength with increased pre-straining and a reduced effect on deformability.

[0113] Figure 29 shows an increase in yield strength (referred to as "Rp") with increasing pre-straining. Figure 29 also shows a decrease in elongation (referred to as "A80") with increasing pre-straining. Applying a PFHT step provided increased strength with increased pre-straining and a reduced effect on deformability. Combining pre-straining and PFHT exhibited a partial restoration of deformability.

[0114] Figures 30 and 31 show increases in both yield strength (Figure 30) and ultimate tensile strength (Figure 31) after various pre-straining and various PFHT procedures. The PFHT procedures included heating the alloys for 30 minutes at a temperature ranging from 195 °C to 215 °C, as indicated in the figures. Yield strengths greater than 300 MPa were achieved after PFHT of aluminum alloys subjected to 0 %, 2 %, 5 %, and 10 % pre-straining (see Figure 30). Ultimate tensile strengths greater than 370 MPa were achieved after PFHT of aluminum alloys subjected to 0 %, 2 %, 5 %, and 10 % pre-straining (see Figure 31). Figures 30 and 31 show a significant increase in both yield strength and ultimate tensile strength after PFHT for all pre-strained aluminum alloys.

[0115] Figures 32 and 33 show decreases in both elongation (Figure 32) and bend angle (Figure 33) after various pre-straining and various PFHT procedures. A percent elongation of greater than 11 % was achieved after PFHT of aluminum alloys subjected to 0 %, 2 %, 5 %, and 10 % pre-straining (see Figure 32). Bend angles greater than 50° were achieved after PFHT of aluminum alloys subjected to 0 %, 2 %, 5 %, and 10 % pre-straining (see Figure 33). Figures 32 and 33 show that there was no significant degradation of deformability in the pre-strained and post-forming heat treated aluminum alloys. Aluminum alloys pre-strained and not subjected to the PFHT, however, do show greater deformability. Surprisingly, all pre-strained aluminum alloys exhibited similar elongation (see Figure 32) and bendability (see Figure 33) after PFHT.

[0116] Figures 34 and 35 show the changes in deformability and yield strength after various pre-straining and PFHT performed at various temperatures for 30 minutes. Aluminum alloy samples subjected to pre-straining without PFHT are indicated by solid symbols. Aluminum alloy AA7075 samples subjected to pre-straining with PFHT are indicated by open symbols and connecting lines. Figure 34 shows an increase in yield strength (referred to as "Rp") with increasing pre-straining. Figure 34 also shows a decrease in bend angle (referred to as "DC alpha 2mm") with increasing pre-straining. Applying a 2% pre-strain and a PFHT step provided increased strength insignificant effect on deformability, suggesting good crashability. Applying a 5% pre-strain and a PFHT softened the alloy and adversely affecting formability and crashability. Figure 35 shows an increase in yield strength (referred to as "Rp") with increasing pre-straining. Figure 35 also shows a decrease in elongation (referred to as "A80") with increasing pre-straining. Applying a PFHT step provided increased strength with increased pre-straining and an adverse effect on deformability. Combining pre-straining and PFHT exhibited a partial restoration of deformability.

[0117] Figures 36 and 37 show the effects of a 2% pre-strain on yield strength (Figure 36) and elongation (Figure 37) on an AA7075 aluminum alloy in T4 temper after various paint baking procedures. As evident in the example of Figure 36, the 2% pre-straining procedure increased yield strength in the AA7075 aluminum alloy regardless of subsequent paint baking procedure. As evident in Figure 37, the 2% pre-straining procedure decreased the formability of the AA7075 aluminum alloy after the paint baking procedure.


Claims

1. A method of producing an aluminum alloy metal product, the method comprising;

casting an aluminum alloy to form a cast aluminum alloy product, wherein the aluminum alloy comprises 0.25 - 1.1 wt. % Cu, 0.6 - 1.1 wt. % Si, 0.7 - 1.2 wt. % Mg, up to 0.25 wt. % Cr, up to 0.35 wt. % Mn, up to 0.4 wt. % Fe, up to 0.25 wt. % Zr, from 0.06 to 0.3 wt. % Zn, up to 0.30 wt. % Ti, up to 0.04 wt. % Ni, and up to 0.15 wt. % of impurities, with the remainder as Al;

homogenizing the cast aluminum alloy product by heating to a temperature from 520°C to 580°C with a soaking time from 30 minutes to 18 hours;

hot rolling the cast aluminum alloy product to produce a sheet, plate, or shate with a hot mill entry temperature of 440°C to 540°C and a hot roll exit temperature of 250°C to 380°C;

solutionizing the sheet, plate, or shate at a temperature between 520 °C and 580 °C and then quenching at a quench rate from 50°C/s to 400°C/s;

pre-aging the sheet, plate, or shate, wherein the pre-aging comprises heating the sheet, plate or shate to a pre-aging temperature of 115°C to 135°C after solutionizing and soaking at the pre-aging temperature for a period of time; and

coiling the sheet, plate, or shate.


 
2. The method of claim 1, wherein the aluminum alloy comprises 0.6 - 1.1 wt. % Cu, 0.6 - 1.1 wt. % Si, 0.7 - 1.2 wt. % Mg, up to 0.25 wt. % Cr, up to 0.35 wt. % Mn, 0.05 - 0.4 wt. % Fe, up to 0.25 wt. % Zr, from 0.06 to 0.3 wt. % Zn, up to 0.10 wt. % Ti, up to 0.04 wt. % Ni, and up to 0.15 wt. % of impurities, with the remainder as Al.
 
3. The method of claim 1, wherein the aluminum alloy comprises 0.75 - 0.9 wt. % Cu, 0.65 - 0.9 wt. % Si, 0.85 - 1.0 wt. % Mg, 0.05 - 0.18 wt. % Cr, 0.05 - 0.18 wt. % Mn, 0.12 - 0.3 wt. % Fe, up to 0.15 wt. % Zr, from 0.06 to 0.1 wt. % Zn, 0.01 - 0.04 wt. % Ti, up to 0.034 wt. % Ni, and up to 0.15 wt. % of impurities, with the remainder as Al.
 
4. The method of any one of claims 1-3, wherein the pre-aging comprises heating the sheet, plate, or shate to a temperature of 120 °C to 130 °C after solutionizing.
 
5. The method of any one of claims 1-4, further comprising strain hardening and thermal treating.
 
6. The method of claim 5, wherein the strain hardening comprises 2% and the thermal treating comprises maintaining the aluminum alloy metal product at a temperature of 185 °C for a time period of 20 minutes.
 
7. The method of any one of claims 1-4, further comprising a thermal treatment of maintaining the aluminum alloy metal product at a temperature of 185 °C for a time period of 20 minutes.
 
8. The method of any one of claims 1-7, further comprising cold rolling the aluminum alloy metal product.
 
9. The method of any one of claims 1-8, further comprising aging the aluminum alloy metal product, wherein the aging comprises heating the aluminum alloy metal product between 180 °C to 225 °C for a period of time.
 
10. The method of any one of claim 1-9, further comprising pre-straining the aluminum alloy metal product, wherein the pre-straining comprises applying a tensile strain to the aluminum alloy metal product after solutionizing.
 
11. An aluminum alloy metal product, wherein the aluminum alloy metal product is prepared by a method of any one of claims 1-10.
 
12. The aluminum alloy metal product of claim 11, wherein the aluminum alloy product comprises a transportation body part.
 
13. The aluminum alloy metal product of claim 12, wherein the transportation body part comprises an automotive body part or a structural body part.
 
14. The aluminum alloy metal product of claim 11, wherein the aluminum alloy product comprises an electronics device housing.
 


Ansprüche

1. Verfahren zur Herstellung eines Aluminiumlegierungmetallprodukts, wobei das Verfahren umfasst:

Gießen einer Aluminiumlegierung, um ein Aluminiumlegierungsgussprodukt zu bilden, worin die Aluminiumlegierung 0,25 - 1,1 Gew.-% Cu, 0,6 - 1,1 Gew-% Si, 0,7 - 1,2 Gew.-% Mg, bis zu 0,25 Gew.-% Cr, bis zu 0,35 Gew.-% Mn, bis zu 0,4 Gew.-% Fe, bis zu 0,25 Gew.-% Zr, 0,06 bis 0,3 Gew.-% Zn, bis zu 0,30 Gew.-% Ti, bis zu 0,04 Gew.-% Ni und bis zu 0,15 Gew.-% Verunreinigungen enthält, wobei der Rest Al ist,

Homogenisieren des Aluminiumlegierungsgussprodukts durch Erwärmen auf eine Temperatur von 520 °C bis 580 °C mit einer Durchwärmungszeit von 30 Minuten bis 18 Stunden;

Warmwalzen des Aluminiumlegierungsgussprodukts zur Herstellung eines Blechs, einer Platte oder eines Shate mit einer Warmwalzeneintrittstemperatur von 440 °C bis 540 °C und einer Warmwalzenaustrittstemperatur von 250 °C bis 380 °C,

Lösungsglühen des Blechs, der Platte oder des Shate bei einer Temperatur zwischen 520 °C und 580 °C und anschließendes Abschrecken mit einer Abschreckgeschwindigkeit von 50 °C/s bis 400 °C/s;

Voraltern des Blechs, der Platte oder des Shate, wobei das Voraltern das Erwärmen des Blechs, der Platte oder des Shate auf eine Voralterungstemperatur von 115 °C bis 135 °C nach dem Lösungsglühen und dem Durchwärmen bei der Voralterungstemperatur für eine Zeitspanne umfasst; und Aufwickeln des Blechs, der Platte oder des Shate.


 
2. Verfahren nach Anspruch 1, worin die Aluminiumlegierung 0,6 - 1,1 Gew.-% Cu, 0,6 - 1,1 Gew.-% Si, 0,7 - 1,2 Gew.-% Mg, bis zu 0,25 Gew.-% Cr, bis zu 0,35 Gew.-% Mn, 0,05 - 0,4 Gew.-% Fe, bis zu 0,25 Gew.-% Zr, 0,06 bis 0,3 Gew.-% Zn, bis zu 0,10 Gew.-% Ti, bis zu 0,04 Gew.-% Ni und bis zu 0,15 Gew.-% Verunreinigungen enthält, wobei der Rest Al ist.
 
3. Verfahren nach Anspruch 1, worin die Aluminiumlegierung 0,75 - 0,9 Gew.-% Cu, 0,65 - 0,9 Gew.-% Si, 0,85 - 1,0 Gew.-% Mg, 0,05 - 0,18 Gew.-% Cr, 0,05 - 0,18 Gew.-% Mn, 0,12 - 0,3 Gew.-% Fe, bis zu 0,15 Gew.-% Zr, von 0,06 bis 0,1 Gew.-% Zn, 0,01 - 0,04 Gew.-% Ti, bis zu 0,034 Gew.-% Ni und bis zu 0,15 Gew.-% Verunreinigungen enthält, wobei der Rest Al ist.
 
4. Verfahren nach einem der Ansprüche 1 bis 3, worin die Voralterung das Erwärmen des Blechs, der Platte oder des Shate auf eine Temperatur von 120 °C bis 130 °C nach dem Lösungsglühen umfasst.
 
5. Verfahren nach einem der Ansprüche 1 bis 4, das außerdem Kalthärten und Wärmebehandlung umfasst.
 
6. Verfahren nach Anspruch 5, worin die Kalthärtung 2 % umfasst und die Wärmebehandlung das Halten des Aluminiumlegierungsmetallprodukts bei einer Temperatur von 185 °C über eine Zeitdauer von 20 Minuten umfasst.
 
7. Verfahren nach einem der Ansprüche 1 bis 4, das weiterhin eine thermische Behandlung umfasst, bei der das Aluminiumlegierungsmetallprodukt über einen Zeitraum von 20 Minuten auf einer Temperatur von 185 °C gehalten wird.
 
8. Verfahren nach einem der Ansprüche 1-7, das weiterhin das Kaltwalzen des Aluminiumlegierungsmetallprodukts umfasst.
 
9. Verfahren nach einem der Ansprüche 1 bis 8, weiterhin umfassend das Altern des Aluminiumlegierungsmetallprodukts, wobei das Altern das Erwärmen des Aluminiumlegierungsmetallprodukts bei 180 °C bis 225 °C über einen Zeitraum umfasst.
 
10. Verfahren nach einem der Ansprüche 1 bis 9, weiterhin umfassend das Vorspannen des Aluminiumlegierungsmetallprodukts, wobei das Vorspannen das Anwenden einer Zugspannung auf das Aluminiumlegierungsmetallprodukt nach dem Lösungsglühen umfasst.
 
11. Aluminiumlegierungsmetallprodukt, wobei das Aluminiumlegierungsmetallprodukt nach einem Verfahren nach einem der Ansprüche 1-10 hergestellt ist.
 
12. Aluminiumlegierungsmetallprodukt nach Anspruch 11, wobei das Aluminiumlegierungsprodukt ein Karosserieteil eines Verkehrsmittels umfasst.
 
13. Aluminiumlegierungsmetallprodukt nach Anspruch 12, wobei das Karosserieteil eines Verkehrsmittels ein Kraftfahrzeugkarosserieteil oder ein Strukturkarosserieteil umfasst.
 
14. Aluminiumlegierungsmetallprodukt nach Anspruch 11, wobei das Aluminiumlegierungsprodukt ein Gehäuse für ein elektronisches Gerät umfasst.
 


Revendications

1. Procédé de production d'un produit métallique en alliage d'aluminium, le procédé comprenant ;

le coulage d'un alliage d'aluminium pour former un produit coulé en alliage d'aluminium, dans lequel l'alliage d'aluminium comprend 0,25 à 1,1 % en poids de Cu, 0,6 à 1,1 % en poids de Si, 0,7 à 1,2 % en poids de Mg, jusqu'à 0,25 % en poids de Cr, jusqu'à 0,35 % en poids de Mn, jusqu'à 0,4 % en poids de Fe, jusqu'à 0,25 % en poids de Zr, de 0,06 à 0,3 % en poids de Zn, jusqu'à 0,30% en poids de Ti, jusqu'à 0,04 % en poids de Ni, et jusqu'à 0,15 % en poids d'impuretés, le reste étant de l'Al ;

l'homogénéisation du produit coulé en alliage d'aluminium par chauffage à une température de 520 °C à 580 °C avec un temps d'égalisation de 30 minutes à 18 heures ;

le laminage à chaud du produit coulé en alliage d'aluminium pour produire une feuille, une plaque ou un feuillard avec une température d'entrée de laminoir à chaud de 440 °C à 540 °C et une température de sortie de rouleau chaud de 250 °C à 380 °C ;

la mise en solution de la feuille, de la plaque ou du feuillard à une température entre 520 °C et 580 °C et ensuite la trempe à une vitesse de trempe de 50 °C/s à 400 °C/s ; le pré-vieillissement de la feuille, de la plaque ou du feuillard, dans lequel le pré-vieillissement comprend le chauffage de la feuille, de la plaque ou du feuillard à une température de pré-vieillissement de 115 °C à 135 °C après mise en solution et égalisation à la température de pré-vieillissement pendant une période de temps ; et le bobinage de la feuille, de la plaque ou du feuillard.


 
2. Procédé selon la revendication 1, dans lequel l'alliage d'aluminium comprend 0,6 à 1,1 % en poids de Cu, 0,6 à 1,1 % en poids de Si, 0,7 à 1,2 % en poids de Mg, jusqu'à 0,25 % en poids de Cr, jusqu'à 0,35 % en poids de Mn, 0,05 à 0,4 % en poids de Fe, jusqu'à 0,25 % en poids de Zr, de 0,06 à 0,3 % en poids de Zn, jusqu'à 0,10 % en poids de Ti, jusqu'à 0,04% en poids de Ni, et jusqu'à 0,15 % en poids d'impuretés, le reste étant de l'Al.
 
3. Procédé selon la revendication 1, dans lequel l'alliage d'aluminium comprend 0,75 à 0,9 % en poids de Cu, 0,65 à 0,9 % en poids de Si, 0,85 à 1,0 % en poids de Mg, 0,05 à 0,18 % en poids de Cr, 0,05 à 0,18 % en poids de Mn, 0,12 à 0,3 % en poids de Fe, jusqu'à 0,15 % en poids de Zr, de 0,06 à 0,1 % en poids de Zn, 0,01 à 0,04 % en poids de Ti, jusqu'à 0,034 % en poids de Ni, et jusqu'à 0,15 % en poids d'impuretés, le reste étant de l'Al.
 
4. Procédé selon l'une quelconque des revendications 1 à 3, dans lequel le pré-vieillissement comprend le chauffage de la feuille, de la plaque ou du feuillard à une température de 120 °C à 130 °C après mise en solution.
 
5. Procédé selon l'une quelconque des revendications 1 à 4, comprenant en outre un écrouissage et un traitement thermique.
 
6. Procédé selon la revendication 5, dans lequel l'écrouissage comprend 2 % et le traitement thermique comprend le maintien du produit métallique en alliage d'aluminium à une température de 185 °C pendant une période de temps de 20 minutes.
 
7. Procédé selon l'une quelconque des revendications 1 à 4, comprenant en outre un traitement thermique de maintien du produit métallique en alliage d'aluminium à une température de 185 °C pendant une période de temps de 20 minutes.
 
8. Procédé selon l'une quelconque des revendications 1 à 7, comprenant en outre le laminage à froid du produit métallique en alliage d'aluminium.
 
9. Procédé selon l'une quelconque des revendications 1 à 8, comprenant en outre le vieillissement du produit métallique en alliage d'aluminium, dans lequel le vieillissement comprend le chauffage du produit métallique en alliage d'aluminium entre 180 °C à 225 °C pendant une période de temps.
 
10. Procédé selon l'une quelconque des revendications 1 à 9, comprenant en outre la pré-contrainte du produit métallique en alliage d'aluminium, dans lequel la pré-contrainte comprend l'application d'une contrainte de traction sur le produit métallique en alliage d'aluminium après mise en solution.
 
11. Produit métallique en alliage d'aluminium, dans lequel le produit métallique en alliage d'aluminium est préparé par un procédé selon l'une quelconque des revendications 1 à 10.
 
12. Produit métallique en alliage d'aluminium selon la revendication 11, dans lequel le produit en alliage d'aluminium comprend une pièce de corps de transport.
 
13. Produit métallique en alliage d'aluminium selon la revendication 12, dans lequel la pièce de corps de transport comprend une pièce de carrosserie d'automobile ou une pièce de corps structural.
 
14. Produit métallique en alliage d'aluminium selon la revendication 11, dans lequel le produit en alliage d'aluminium comprend un boîtier de dispositif électronique.
 




Drawing

















































































































Cited references

REFERENCES CITED IN THE DESCRIPTION



This list of references cited by the applicant is for the reader's convenience only. It does not form part of the European patent document. Even though great care has been taken in compiling the references, errors or omissions cannot be excluded and the EPO disclaims all liability in this regard.

Patent documents cited in the description




Non-patent literature cited in the description