/ BACKGROUND OF THE INVENTION
[0001] Thermosetting unsaturated polyester resin based molding compounds are well known
and consist of an unsaturated polyester resin, an ethylenically unsaturated copolymerizable
monomer, inert mineral fillers, fibrous reinforcing fillers and a catalyst which initiates
the cross-linking reaction between the copolymerizable monomer and the unsaturated
polyester resin at a chosen molding temperature. They are commonly used in many physical
forms two of which are bulk molding compounds (BMC) and sheet molding compounds (SMC).
In bulk molding compounds, the fibrous reinforcing filler which is normally about
0.25 inch in length, is mechanically mixed with the unsaturated resin. In sheet molding
compounds, the fibrous reinforcing filler which is normally about 0.5 to 2 inches
in length, is present as chopped fibers deposited on a supporting carrier which are
impregnated with the unsaturated resin system, giving rise to sheets of molding compound
in which the fibers have not been subjected to the degrading action of conventional
molding compound mixers.
[0002] The use of unsaturated polyester resins in the molding of glass fiber reinforced
or other fiber reinforced products enjoys broad application in the manufacture of
automotive, industrial and home products.
[0003] Polyester molding compounds are described in U.S. Patents 3;940,350, 3,974,124, 3,227,665,
3,701,748, and 3,948,716.
[0004] 'Unfortunately, polyester resins are inherently brittle and whenever unsaturated
polyester resins are used as a matrix, then the toughening of the matrix is important.
Normal industry practice is.to add a flexibilizer to the resin composition which often
results in a significant reduction in the mechanical properties. This reduction in
mechanical properties is unacceptable for many product applications. It is desirable
to toughen unsaturated polyester resin compositions without significant adverse effects
on other important properties such as cure rate, maturation and strength.
SUMMARY OF THE INVENTION
[0005] To an unsaturated polyester molding composition containing unsaturated polyester
resin(s), and polymerizable monomer(s) is added from about 1 to about 30 parts by
weight of an epihalohydrin polymer per 100 parts by weight of the combined weight
of the polyester resin and the polymerizable monomer. The composition containing the
epihalohydrin polymer is greatly improved for toughness without significant adverse
effects on strength and processing characteristics such as cure rate and maturation.
DETAILED DESCRIPTION
[0006] Polyesters useful in this invention are well known in the art and include those derived
by conden.sation of unsaturated dibasic acids or anhydrides containing 4 to 9 carbon
atoms with polyols including dihydroxy and trihydroxy compounds containing 2 to 12
carbon atoms. The polyester may include the polymeric chain varying proportions of
other saturated or aromatic dibasic acids and anhydrides which are not subject to
cross-linking. The particular noncrosslinking moieties and their proportions will
depend upon the desired properties of the final product. Maleic, chloromaleic and
fumaric acid may be mentioned as exemplary of noncrosslinking moieties within the
copolymer include: phthalic anhydride, endomethylene-tetrahydrophthalic acid, tetrachlorophthalic
acid, hexachloroendomethylenetetrahydrophtha.ic acid, adipic acid, sebacic acid, succinic
acid, and the like.
[0007] Any of a variety of well known polyols including di- and tri- hydroxy compounds containing
4 to 9 carbon at ms, preferably 4 to 6 carbon atoms can be used for condensation with
the diacids to produce polyesters suitable for use i this invention. Preferred compounds,
which are mentioned oy way of example, of the large number of applicable compouns
include: ethylene glycol, diethylene glycol, propylene glycol, polypropylene glycol,
glycerol, 1,2-, 1,3-, and ,4-butadienols, trimethylol propane, and the like. The method
by which the unsaturated polyester resins are made is rot critical to this invention.
[0008] The polyester resin is dissolved in a solven comprising at least one polymerizable
monomer which is co oly- merizable with the dissolved polyester. The

monomer not only acts as a solvent but also

with the unsaturated groups alons the polyester

Polymerizable monomers which can be used in this invention include polymerizable vinylidene
compounds having at least one terminal CH
2 < group and cantaining 2 to 12 carban andpreferably 3 to 10 carbon atoms. A wide
variety of thesse compounds are known including both aliphatic and aromatic unsaturated
hydrocarbons and hydzcocarbon derivatives, suchas esters, acids and nitriles. Examples
of suitable polymerizable monomers are styrene, methyl styrene, acrylonitril methyl
acrylate, methyl methacrylate, vinyl dcetate, allyl esters of phthalic, adipic, maleic,
malonic, andoyanuricacids. Styrene and methyl styrene are particularly useful polymerizable
monomers. Commercial unsaturated polyester resins are normally sold as a liquid solution
with the unsaturated polyester resin dissolved in the polymerizable monomer.
[0009] Epihalohydrin polymers used as toughners in thisinvention can be an epihalohydrin
homopolymer, a copolymor or two or more epihalohydrin monomers, or a copolymer of

halohydrin monomer(s) with an oxide monomer(s).
[0010] The epihalohydrin monomers have the formula

where X is Cl, Br, I, or F. More preferredly, X is selectedfrom Cl and Br. From a
cost and availability standpoint the preferred monomer is epichlorohydrin. Other halogen-bearing
epoxide monomers can be used in partial replacement of the epihalohydrin monomer(s).
Examples of these monomers are 4-chloro-1,2-epoxy butane; 4-bromo-1, 2-epoxy butane:
1-(1,3-dichloroisopropoxy)-2,3,-epoxypropane; 4,4,4-trichoro-1-2-epoxy butane; 1-bromoethyl
glyaidyl ether; 1,1,1-trichloro-ethyl glycidyl ether; 1,1,1-trifluoroethyl glycidyl

1,2-epoxy-2-meth-6,6,6,6-

8,8,8,-trichloro

[0011] The oxide monomers contain a cyclic oxy

ring therein. Examples of these monomers are alkylene oxides such as ethylene oxide,
propylene oxide, butylene oxide, isobutylene oxide, octylene oxide, and the like;
cycloaliphatic oxides such as cyclohexene oxide, vinyl cyclohexene oxide, and the
like; glycidyl ethers such as methyl glycidyl ether, ethyl glycidyl ether, isopropyl
glycidyl ether, n-hexyl glycidyl ether, phenyl glycidyl ether and the like; glycidyl
acrylate and glycidyl methacrylate; allyl glycidyl ether; styrene oxide; and 4- and
5- membered oxy ring compounds such as Furan and methyl substituted Furan, and the
like. Of the oxide monomers, the alkylene oxides containing two to about eight carbon
atoms are preferred.
[0012] Examples of more preferred epihalohydrin polymers are polyepichlorohydrin, polyepibromohydrin,
epichlorohydrin- epibromohydrin copolymer, epichlorohydrin-ethylene oxide copolymer,
epibromohydrinethylene oxide copolymer, epichlorohydrin-propylene oxide copolymer,
and epichlorohydrin-ethylene oxidepropylene oxide terpolymer. Excellent results have
been obtained with a homopolymer of epichlorohydrin.
[0013] Copolymers of epihalohydrin monomers and oxide monomers comprise at least 50% to
100% by weight (i.e., homopolymers) of polymerized units of epihalohydrin monomer(s),
and up to 50% by weight of polymerized units of an oxide monomer(s). Preferably, the
polymers contain from about 65% to 100% by weight of polymerized epihalohydrin monomer(s).
[0014] Epihalohydrin polymers suitable for use as tougheners for unsaturated polyester resins
are of low molecular weight and will vary in form from fluid liquids to thick semisolids.
The number average molecular weight (Mn) of such, polymers normally will vary from
about 800 to about 50,000, preferably from about 2000 to about 15,000. The molecular
weight is normally specified in terms of "Reduced Solution Viscosity" or "RSV" which
is a point value viscosity determined as the viscosity at 25°C of a solution of 0.4
gram of polymer dissolved in 100 ml. of dimethyl formamide containing 3% by volume
of acetylacetone expressed as decaliter per gram or dl./g.l. The range of RSV corresponding
to the. number average molecular weight range given above will be from about 0.025
to about 0.5, preferably from about 0.075 to about 0.3. The epihalohydrin polymers
have a bulk viscosity of from about 500 cps. to about 50,000,000 cps (measured at
27°C using a Brookfield Viscometer). To facilitate handling the bulk viscosity of
the epihalohydrin polymer can be reduced by blending the polymer with the dissolving
polymerizable monomer. This may be desirable for high viscosity polymers. Liquid epichlorohydrin
polymers were found to be excellent tougheners for unsaturated polyester resins.
[0015] Epihalohydrin polymers suitable for use in this invention can be prepared according
to U.S. Patent 3,850,856 (incorporated herein by reference) and U.S. Patent 3,850,857
(incorporated herein by reference).
[0016] The level of epihalohydrin polymer(s) used is from about 1 to about 30 parts by weight,
preferably from about 1 to about 15 parts by weight, said weight parts being based
on 100 parts by weight of the polyester resin and the polymerizable monomer.
[0017] In addition to the polyester resin, the polymerizable monomer and the epihalohydrin
polymer, the molding compositions of this invention may include other ingredients
such as fillers, mold lubricants, catalysts, thickening agents, low profile additives,
reinforcing fibers, flame and smoke retardants, and coloring agents.
[0018] As regards the filler materials suitable for use in the compositions of this invention,
these may include conventional inorganic fillers such as carbonates, sulfates, phosphates,
silica, silicate, micromica, carborundum, asbestos, glass, sandstone, graphite and
the like reduced to a fine powder, as well as organic materials such as polyolefins,
polyvinyl chloride, carbon black and acetylene black, polyacrylate, polymethacrylates,
solid polyesters, phenol-formaldehyde resins, urea-formaldehyde resins, polyformol
resins, polyamid resins, used in powder of appropriate granulbmetric compositon ranging
from very fine powder to granular size. The particles may somethmes fuse during the
final cross-linking process.
[0019] Organic or inorganic bubbles may be used as fillers to reduce the weight of the unsaturated
polyester compositions. Hollow glass bubbles are particularly desirable as a weight
reducing filler. The glass bubbles have a nominal density less than 0.7 and preferably
less than 0.5 gram per cubic centimeters. They are of small particle size of from
about 1 to about 500 microns and preferably less than 150 microns.
[0020] As reinforcing fibers, there may be used inorganic fibers such as glass fibers, asbestos
fibers; vegetable fibers such as flax, hemp, cotton, and the like; and organic fibers
such as nylon, polyester, aromatic polyamide and the like. The reinforcing fibers
may be present as chopped fibers having lengths of from about 0.1 to about 3 inches
or as woven mats, non-woven mats and the like. Sheet molding compounds will normally
have chopped fibers of from about 0.5 to about 2 inches. The quantity of reinforcing
fibers used will normally be from about 5 to 70 percent, preferably from 15 to 50
percent of fibers of the total weight of the composition.
[0021] Mold lubricants which may be employed in the preparation of the compositions of this
invention include mold lubricants well known in the art and the choice is not critical.
There may be mentioned, by way of example, zinc stearate, calcium or magnesium stearate
or oleate and zinc oleate. In some instances, the mold lubricant may be omitted as
where organic fillers having the property of being self- lubricating, such as polyolefins,
polyvinylchloride and the like are employed.
[0022] Known chemical thickeners are the oxides and hydroxides of the metals of main group
2 of the periodic system, preferably the oxides and hydroxides of magnesium and calcium,
to which small amounts of water are added optionally. Magnesium oxide was found to
be an especially desirable thickener. The thickeners are normally used at levels of
from about 1 to about 3 parts by weight per 100 parts of the combined weight of polyester
resin and polymerizable monomer..
[0023] Examples of suitable catalysts are benzoyl peroxide, tertiary butyl peroxide, cyclohexanone
peroxide, tertiary butyl peroctoate, tertiary butyl perbenzoate,

dinitrile, cumene hydroperoxide and the like. The catalysts are normally used at levels
of from about 0.5 to about 3 parts by weight per 100 parts of the combined weight
of polyester resin and polymerizable monomer.
[0024] Many applications for which unsaturated polyester compositions are used are not critical
with respect to surface smoothness, but in certain uses such as automobile surface
parts, for example, the characteristic rough surface is objectionable. Often it is
desirable to paint moldings used in automotive applications, for example, to achieve
a smooth, metal-like, high-gloss appearance. To achieva a smooth surface, it is customary
to use a low shrink additive, which is commonly referred to as a low-profile additive.
Low-profile additives are widely used in sheet molding compounds.
[0025] Low-profile additives which may be used in the unsaturated polyester resin compositions
of this invention are well known in the art. They include thermoplastic homopolymers
of vinylidene monomers containing 2 to 12 carbon atoms. Examples are homopolymers
of alkyl acrylates and methacrylates such as methyl acrylate, ethyl acrylate, methyl
methacrylate, ethyl methacrylate, butyl methacrylate and the like; vinyl esters such
as vinyl acetate and the like; vinyl halides such as vinyl chloride and the like;
vinyl aromatics such as styrene and the like. Thermoplastic copolymers are also suitable
for use as a low-profile additive such as copolymers of methyl methacrylate and lower
alkyl esters of acrylic and methacrylic acids, and copolymers of methyl methacrylate
with minor amounts of one or more of the following: lauroyl methacrylate, isobornyl
methacrylate, acrylamide, hydroxyethyl methacrylate, styrene, 2-ethylhexyl acrylate,
acrylonitrile, methacrylic acid, methaorylamide, methylol acrylamide and cetyl stearyl
methacrylate. Copolymers of Vinyl halides and vinyl esters are also useful as low-profile
additives such as vinyl chloride/vinyl acetate copolymers and the like. Other useful
examples of low-profile additives are styrene/acrylonitrile copolymers, cellulose
acetate butyrate, and cellulose acetate propionate. Excellent results were obtained
using polyvinyl acetate.
[0026] Low-profile additives are normally supplied in a solution with a polymerizable monomer
such as styrene. After cure, the low-profile additive exists as fine particles dispersed
in the polyester matrix. Low-profile additives may be used at a level of from about
5 to about 40 parts by weight based on 100 parts by weight of the combined weight
of the unsaturated polyester resin and the polymerizable monomer.
[0027] To prepare the novel molding compositions of this invention, normal procedures for
preparing unsaturated polyester molding compositions are used except that the epihalohydrin
liquid polymer is mixed with the polyester resin and polymerizable monomer. The remainder
of the preparation procedure will vary somewhat depending on the type of molding composition
desired, such as sheet molding, bulk molding, hand lay-up, spray-up, vacuum bag molding,
injection molding, casting and the like.
[0028] For sheet molding compounds a typical preparation procedure is to first mix the liquid
ingredients together, that is the unsaturated polyester resin, polymerizable monomer,
low-profile additive and the epihalohydrin polymer. The epihalohydrin polymer may
be added as is or mixed with the polymerizable monomer to reduce its viscosity and
facilitate handling. The liquid ingredients are then mixed with the fillers and mold
release agents for about 15 to 20 minutes in a mixer such as a Cowles mixer. The catalyst
is then added to the mix and mixed for about 2 to 5 minutes. The thickening agent
is then added and mixed for about 1 to 3 minutes. The resin composition is then spread
onto non- adhering sheets such as polyethylene. Chopped glass fibers are then sprayed
onto the sheets of resin compound and the sheets brought together to form a composite.
The composite is passed through compression rollers to effect impregnation of the
glass by the resin mix. The sheets of the composite are then allowed to thicken with
time (maturation) for about 1 to 3 days at about 32°C. For sheet molding-applications,
the resin composition should thicken to a yiscosity of from 6 6 about 30 x 10 cps.
to about 100 x 10 cps
. Preferably from about 50 x 10 cps. to about 70 x 10 cps. before molding under heat
and pressure. The thickened sheets are then cut into the desired size and molded and
cured at an elevated temperature.
[0029] Initial compatibility of the polymer with the polyester resin and polymerizable monomer
is important to produce the desired morphology. Quite unexpectedly, it was found that
when the epihalohydrin polymer is mixed with the polyester resin and the polymerizable
monomer, the polymer appears to dissolve and becomes compatible with the mix. This
phenomenon is unusual since other liquid polymers such as liquid acrylonitrile/butadiene
polymer would not readily dissolve in the resin mix. When the rubber polymer is incompatible
with the resin mix, there can be no control of rubber particle size beyond mixing
conditions and speed of processing. Therefore, the rubber domains are large (greater
than 10 microns). When the compatible epihalohydrin polymer is used as a toughener
for polyester resins, the rubber domains are very small (from submicron to 10 microns
in size) which is desirable for toughness improvement. The unexpectedly small particles
of epihalchydrin polymer in the polyester is believed to result from its compatibility
and subsequent precipitation at the onset of resin gelation.
[0030] Since the epihalohydrin is compatible with the unsaturated polyester resin mix, the
compositions of this invention have excellent storage properties. When an incompatible
polymer is used in the mix and the mix is not used within a short time after mixing,
the polymer has a tendency to separate from the mix. The epihalohydrin, polyester
resin and polymerizable monomer of this invention can be premixed and stored for long
periods of time before the catalyst and thickening agent are added to the mix. This
is a very desirable feature for unsaturated polyester molding compositions.
[0031] In order to evaluate the compositions of this invention for toughness and other properties,
standard industry tests may be used. ASTM tests can be used for conventional mechanical
properties such as D-790 for flexure and D-638 for tension, both with nominal 6.35
mm thick samples. Izod testing was done un samples that were unnotched and impacted
normal to the molding surface. Other tests were used to measure shrinkage in the mold
and Barcol hardness. Fracture toughness was evaluated by the Gardner dart impact test
and by an acoustic emission test designed to measure . crack development during bending.
The Gardner impact and acoustic emission tests warrant more detailed description.
[0032] For the Gardner impact test, an instrument is used which comprises a base plate,
a round-nosed steel rod impact weight, a slotted tube having inch-pound graduations
in which the rod is lifted and dropped, and a bracket to hold the tube in a vertical
position. Impact resistance is determined by sujecting either side of a sample panel
to an impact of up to 320 inch-pounds, depending upon the weight dropped. The sample
panel is placed over a 12.7 mm hole in the base plate; the steel rod weight is raised
by lifting an attached pin until the pin coincides with the desired inch-pounds graduation
mark on the slotted tube, and then dropped. The sample panel is examined for cracking
or failure after each impact. The test used a 1.59 mm radius dart on a 6.35 mm sample
panel. A two-pound weight was dropped from various heights onto the ring supported
sample. The resultant damage was determined by detecting cracking on the reverse side
of the sample. The detection was made relatively easy by inking the reverse side and
then wiping it clean; the ink clearly identified the local cracking from the impact.
The dart weight multiplied by the drop height at the onset of detectable cracking
determined the reported Gardner impact value in inch-pounds.
[0033] The acoustic emission test was devised to measure cracking during a simple cantilever
bending load. In it, a 3.18 mm thick sample, 38 mm wide and 127 mm long is mounted
in a Tinius Olsen Stiffness Tester and bent by applying a weight.of 22.7 kg. The sample
bent until 70% of the weight was applied to it. The load caused the sample to bend
through 6 - 7° of measured arc. A dynamic microphone was mounted in contact with the
specimen at the point of maximum arc. A tape recorder was used to record the noise
of crack development during the bending sequence. This record can be played back for
an audible comparison of different samples. At the same time, the tape output can
be fed into an oscillo scope for a visible record of the cracking noise. The oscilloscope
trace can be photographed to record the test. A numerical value for the acoustic emission
test is determined by counting the number of peaks from the oscilloscope trace.
[0034] The novel compositions of this invention containing epihalohydrin may be used in
any of the many unsaturated polyester molding applications, but for illustrative purposes,
the examples are directed to unsaturated polyester sheet. molding.
[0035] The following examples illustrate the present invention more fully.
EXAMPLE I
[0036] This example is presented to show the improvement in toughness imparted to an unsaturated
polyester sheet molding compound by the use of a liquid polyepichlorohydrin polymer.
A compound containing no liquid rubber (control) and a compound containing a liquid
acrylonitrile/butadiene rubber (sample 2) are compared with the compound containing
liquid polyepichlorohydrin (sample 1).

[0037] The compositions were prepared by mixing the polyester resin, low-profile additive
(both of which were dissolved in a polymerizable monomer), calcium carbonate, zinc
stearate and liquid polymer (in samples 1 and 2 only). The liquid ingredients (polyester
resin, low-profile additive and rubber) were first mixed together. The liquid ingredients
were then mixed with the calcium carbonate and zinc stearate in a Cowles mixer for
15 minutes and then the t-butyl perbenzoate catalyst was added to the mix and mixing
continued for three minutes. The MgO was then added and mixing continued for two minutes.
The compositions were then spread onto sheets of polyethylene and chopped glass fibers
(1-1/4 inch long) was sprayed onto the compositions. The sheets were brought together
to form a composite. The composite was passed through compression rollers to effect
impregnation of the glass fibers by the resin mix. The quantity of chopped glass fibers
used was such that the final sheet molding compositions were 21% glass. The compositions
were then )rolled up in the polyethylene and allowed to thicken for about 48 hours
at 32°C. The sheets were then cut into sample size and cured for three minutes at
150°C. in a 50 ton press. Testing results are shown in Table II.

[0038] The above test results show that the toughness is greatly improved in the composition
containing epichlorohydrin (sample 1) as is shown by the acoustic emission cracks,
Gardner impact, and Izod impact test results. Other important properties such as tensile
stress and flexure stress are not adversely effected. Processing characteristics such
as shrink, cure rate and maturation are not significantly effected by the use of epichlorohydrin
as a toughener. The significant improvements in Gardner impact and acoustic emissions
were not present in the sample containing the other liquid polymer (sample 2).
EXAMPLE III
[0039] Thisaexample is presented to show the improvement in toughness imparted to a reduced
weight unsaturated polyester sheet molding compound by the use of a liquid polyepichlorohydrin
polymer. The reducedweight compounds contain hollow glass bubbles. The other ingredients
used such as the polyester resin, low-profile additive, fillers and epichlorohydrin
were the same as those used in Example I. The compositions evaluated are shown in
Table III.

[0040] The compositions were prepared as in Example I except that the glass bubbles were
added as a filler along with the calcium carbonate. Testing results are shown in Table
IV.
[0041] As in Example I, the liquid polyepichlorohydrin increased the toughness of the unsaturated
polyoster sheet molding compound without adversely effecting the other properties.
By using polyepichlorohydrin, the acoustio emissions was dramatically reduced (from
40 to 1) which is indictive of the high toughness imparted to sample 4 by the polyepichlorohydrin.
[0042] The unsaturated polyester molding compositions of this invention have many uses including
automotive parts, chairs, trays, and the like.
2. An unsaturated polyester molding composition comprising:
(a) an unsaturated polyester resin,
(b) a polymerizable monomer,
(c) from about 1 to about 30 parts by weight of an epihalohydrin polymer per 100 parts
by weight of the combined weight of said unsaturated polyester resin and polymerizable
monomer.
2. A composition of Claim 1 wherein the epihalohydrin polymer has a number average
molecular weight of from about 800 to about 50,000.
3. A composition of Claim 2 containing a catalytic amount of a catalyst selected from
the group consisting of benzoyl peroxide, tertiary butyl perbenzoate, cyclohexanone
peroxide, tertiary butyl peroxide, tertiary butyl peroctoate, azoisobutyrodinitrile,
and cumene hydroperoxide.
4. A composition of Claim 3 containing fiber reinforcement wherein said fibers are
selected from the group consisting of glass, nylon, polyester, and aromatic polyamide.
5. A composition of Claim 4 wherein the level of said fibers is from about 5 percent
to about 70 percent by weight of the total composition weight.
6. A composition of Claim 4 containing a thermoplastic low-profile additive.
7. A composition of Claim 6 containing as a thickening agent an oxide or hydroxide
of magnesium or calcium.
8. A composition of Claim 7 wherein the low-profile additive is a thermoplastic homopolymer
of a vinylidene monomer containing from 2 to 12 carbon atoms.
9. A composition of Claim 7 wherein said composition has a viscosity of from about
30,000,000 to about 100,000,000 cps.
A composition of Claim 8 wherein the level of epihalohydrin polymer is from about
1 to about 15 parts by weight per 100 parts by weight of the combined weight of said
unsaturated polyester resin and polymerizable monomer.
11. A composition of claim 10 cortaining glass bubbles wherein said glass bubbles
have a density of less than about 0.7 gram per cubic centimeter and a particle size
less than about 500 microns.
12. A composition of Claim 11 wherein the epihalo hydrin polymer is selected from
the group consisting of a homopolymer of an epihalohydrin monomer and a copolymer
of an epihalohydrin monomer and an oxide monomer containing a cyclic oxy ring.
13. A composition of Claim 12 wherein the epihalo- hydrin polymer is a homopolymer of epichlorohydrin.
14. A composition of Claim 13 wherein the fiber reinforcement is chopped glass fiber
having a length of from about 0.1 to about 3 inches.
15. A composition of Claim 3 wherein the epihalohydrin polymer is selected from the
group consisting of a homopolymer of an epihalohydrin monomer and an oxide monomer
containing a cyclic oxy ring.
16. A composition of Claim 15 wherein the level of epihalohydrin polymer is from about
1 to about 15 parts by weight per 100 parts by weight of the combined weight of said
unsaturated polyester resin and polymerizable monomer.
17. A composition of Claim 16 wherein the epihalohydrin polymer is a homopolymer of
epichlorohydrin.
18. A cured composition of Claim 1.
19. A process for producing a moldable unsaturated polyester composition which comprises
mixing at least one unsaturated polyester resin with at least one polymerizable monomer
and from about 1 to about 30 parts by weight of epihalohydrin polymer per 100 parts
by weight of the combined weight of said unsaturated polyester resin and said polymeri-
zable monomer.
20. A process of Claim 19, wherein the epihalohydrin polymer has a number average
molecular weight of from about 800 to about 50,000.
21. A process of Claim 2Q with the added steps of
(a) mixing a catalytic amount of catalyst with the composition,
(b) mixing reinforcing fibers with the composition, and
(c) mixing a thermoplastic low-profile additive with the composition.
22. A process of Claim 21 with the added step of mixing a thickening agent with the
composition wherein said thickening agent is an oxide or hydroxide of magnesium or
calcium.
23. A process of Claim 22 wherein the epihaiohydrin polymer is selected from the group
consisting of a homopolymer of an epihalohydrin monomer and a copolymer of an epihalohydrin
monomer and an oxide monomer containing a cyclic oxy ring, and wherein the level of
said epihalohydrin polymer is from about 1 to about 15 parts by weight per 100 parts
by weight of the combined weight of said unsaturated polyester resin and polymerizable
monomer.
24. A process of Claim 23 wherein the epihalohydrin polymer is a homopolymer of epichlorohydrin.
25. A shaped article comprising:
(a) an unsaturated polyester resin,
(b) a polymerizable monomer, and
(c) from about 1 to about 30 parts by weight of an epihalohydrin polymer per 100 parts
by weight of the combined weight of said unsaturated polyester resin and polymerizable
monomer.
26. An article of Claim 25 wherein the epihalohydrin polymer has a number average
molecular weight of from about 800 to about 50,000.
27. An article of Claim 26 containing fiber reinforcement wherein said fibers are
selected from the group consisting of glass, nylon, polyester and aromatic polyaminde.
28. An article of Claim 27 wherein the level of epihalohydrin polymer is from about
1 to about 15 parts by weight per 100 parts by weight of the combined weight of said
unsaturated polyester resin and polymerizable monomer.
29. An article of Claim 28 containing a thermo- plastic low-profile additive.
30. An article of Claim 29 wherein the epihalohydrin polymer is selected from the
group consisting of a homopolymer of an epihalohydrin monomer and a copolymer of an
epihalohydrin monmer and an oxide monomer containing a cyclic oxy ring.
31. An article of Claim 30 wherein the epihalo- 'hydrin polymer is a homopolymer of
epiohlorohydrin.
32. An article of Claim 31 wherein the fiber reinforcement is chopped glass fiber
having a length of from about 0.1 to about 3 inches.
33. An article of Claim 32 containing, glass bubbles wherein said glass bubbles have
a density of less than about 0.7 gram per cubic centimeter and a particle size less
than about 500 microns.