(19)
(11) EP 0 000 564 A1

(12) EUROPEAN PATENT APPLICATION

(43) Date of publication:
07.02.1979 Bulletin 1979/03

(21) Application number: 78100469.2

(22) Date of filing: 21.07.1978
(51) International Patent Classification (IPC)2: B01J 23/88, B01J 27/18, B01J 27/02, C07C 121/32, C07C 120/14
(84) Designated Contracting States:
BE CH DE FR GB NL SE

(30) Priority: 28.07.1977 US 819732

(71) Applicant: THE STANDARD OIL COMPANY
Cleveland, Ohio 44115 (US)

(72) Inventors:
  • Grasselli, Robert Karl
    Chagrin Falls Ohio 44022 (US)
  • Suresh, Dev Dhanaraj
    Macedonia Ohio 44056 (US)
  • Friedrich, Maria Strada
    Cleveland Ohio 44120 (US)
  • Orndoff, David Allan
    Windsor Ohio 44099 (US)

(74) Representative: Redies, Bernd (DE) et al
Cohausz & Florack Patentanwälte Postfach 14 01 61 Schumannstrasse 97
D-40237 Düsseldorf
D-40237 Düsseldorf (DE)


(56) References cited: : 
   
       


    (54) Catalysts containing iron and molybdenum and the use of these catalysts in the preparation of acrylonitrile or methacrylonitrile


    (57) The invention is related to new catalysts containing iron, bismuth, molybdenum and various additional elements which exhibit extremely attractive catalytic properties for the oxidation and ammoxidation of various olefins. The invention is further related to the use of such catalysts in the ammoxidation of propylene and isobutylene to acrylonitrile and respectively, methacrylonitrile.


    Description

    TECHNICAL FIELD OF THE INVENTION



    [0001] The invention is related to new catalysts sonteining iron, bismuth, molybdenum and various additional elements which exhibit extremely attractive catalytic properties for the oxidation and ammoxidation of various olefins. The invention is further related to the use of such catalysts in the ammoxidation of propylene and isobutylene to acrylonitrile and, respectively, methacrylonitrile.

    BACKGROUND OF THE INVENTION



    [0002] Catalysts for the oxidation, ammoxidation and oxydehydrogenation of olefins are well known. See, for example, U.S. 3,642,930 and U.S. 3,414,631, the disclosures of which are incorporated herein by reference. Further note commonly assigned US-applications Serial No. 490,532 filed July 22, 1974, Serial No. 380,527 filed July 19, 1973, and Serial No. 717,838 filed August 26, 1976, the disclosures of which are also incorporated herein by reference. Although these catalysts of the art are very desirable, the catalysts of the present invention have significant advantages over these other catalysts.

    SUMMARY AND DETAILED DESCRIPTION OF THE INVENTION



    [0003] . The present invention is based on the discovery that certain oxidation catalysts based on iron, bismuth and molybdenum and containing additional specified promoter elements exhibit excellent catalytic activity for a variety of olefin oxidation, ammoxidation, dehydrogenation and oxydehydrogenation reactions. In particular, it has been found that specific catalytic compositions as described below are especially suited for use in producing acrylonitrile and methacrylonitrile by the ammoxidation of propylene and isobutylene, respectively. In addition to being excellent ammoxidation catalysts for the production of acrylonitrile or methacrylonitrile, these catalysts also exhibit excellent catalytic activity for the conversion of olefins having four or more contiguous carbon atoms to the corresponding diolefins, and in the oxydehydrogenation of olefins to diolefins.

    [0004] In accordance with the present invention, novel catalysts having improved catalytic properties are represented by the following empirical formula

    wherein J is an alkali metal, thallium, silver or mixtures thereof;

    Q is Co, Ni, Zn, Cd, Be, Mg, Ca, Sr, Ba, Ra or mixtures thereof;

    Z is a two-or-more element system selected from the group consisting of Ge + Sb, Cu + W, Cu + Sn, Ce + W, Pr + Mn, Sn + Mn, Mn + W,

    W + Sb, Cr + Sn, W + Sn, Ge + Sn, Sb + Sn,

    W + P, Sb + P, Cr + Cu, Mn + Cu, Sb + Cu, Mn + P or mixtures thereof, with the proviso that said catalyst is free of T1 when Z is Mn + P;

    D is Bi or Te; and

    wherein a is 0-5;

    b is 0-20;

    c is greater than 0 to 20;

    d is 0-20;

    e is 0-20; and

    x is a value such that the valence requirement of the elements in the catalyst for oxygen are satisfied.



    [0005] In this catalyst composition, the Z component is composed of systems of two or more specified elements. In these systems as described above, each element of the system is present in an amount of at least 1 atom percent, preferably at least 5 atom percent, based on the atoms in the particular system selected. In this catalyst, D is preferably Bi.

    [0006] Preferably, the catalysts of this invention contains the above-indicated elements in the following amounts:

    a is 0.01 to 0.5,

    b is 0.1 to 20,

    e is 0.1 to 9,

    d is 0.1 to 20, and

    e is 0.1 to 20.



    [0007] Optimally the elements are present in the following amounts:

    a is 0.03 to 0.5,

    b is 4 to 10,

    c is 0.5 to 7,

    d is 0.5 to 5, and

    e is 0.5 to 5.



    [0008] In a particularly preferred embodiment, the foregoing preferred and optimal catalysts contain K. Rb and/or Cs and optionally Ni and/or Co.

    [0009] Also, it is desirable if Z is selected so that the ratio of the amount of the first element of each system as described above to the amount of second element in the system is 1:0.25 to 1:0.75.

    [0010] Of the foregoing catalysts, catalyst in which the Z component is selected from the following combinations of elements are of special interest: Ge + Sb, Cu + W, Cu + Sn, Ce + W, Pr + Mn, Sn + Mn and Mn + W; while those catalysts in which Z is one of Ge + Sb, Cu + W, Cu + Sn, Ce + W and Pr + Mn are particularly noteworthy.

    [0011] The catalysts of this invention can be prepared in any conventional manner known in the art, such as for example the various techniques shown in the patents and applications referred to

    OF THE INVENTION. For example, the catalysts can de made by forming an aqueous composition of decomposable salts and/or oxides of the metals to be incorporated into the catalyst, evaporating the water from the aqueous composition to form a thick paste, drying the thick paste and then calcining the thick paste at elevated temperature in an oxidizing atmosphere. Techniques for forming catalysts of the type described herein are well known in the art, and those skilled in the art should have no difficulty in making catalysts of the invention.

    [0012] The catalysts of the present invention may be used unsupported or supported on various conventional carriers such as Si02, A1203, Zr02, Ti02, BPO4, SbP04, MgO, mont- morillonite, or the like. They may be used in fixed-bed or fluid-bed reactors as desired. When using these catalysts, they are simply substituted for the catalysts previously employed, and the reaction is conducted under substantially the same conditions.

    [0013] For example, when the inventive catalysts are used in the ammoxidation of propylena or isobutylene to form acrylonitrile or methacrylonitrile, respectively, the olefin to be reacted together with oxygen and ammonia in conventional proportions are contacted with the catalyst at an elevated temperature, usually aoout 200-6000C. in a fixed or fluid-bed reactor for a time sufficient to effect the appropriate ammoxidation reaction. Similarly, when the inventive catalysts are employed to catalyze other well known reactions, the reaction conditions employed are those- which are conventional.

    SPECIFIC EMBODIMENTS


    Comparative Example A


    80% K0.1Ni2.5Co4.5Fe3BiP0.5Mo12Ox + 20% SiO2.



    [0014] A solution of 127.1 g. ammonium heptamolybdate (NH4)6Mo7O24·4H2O and water was prepared. To this solution was added 6.9 g. of a 42.5% solution of H3P04 and 102.7 g. of Nalco 40% silica sol to form a slurry. Separately, an aqueous solution containing 72.7 g. ferric nitrate, Fe(NO3)3·-9H20; 29.1 g. bismuth nitrate, Bi(NO3)3·5H2O: 78.6 g. cobalt nitrate Co(NO3)2·6H2O; 43.6 g. nickel nitrate Ni(NO3)2·6H2O: and 6.1 g. of a 10% potassium nitrate solution was prepared. The solution of metal nitrates was slowly added to the slurry. The resulting slurry was evaporated to dryness, and the solid obtained was heat treated at 290°C for three hours, at 425°C for three hours and at 550°C for 16 hours.

    Examples 1 to 7



    [0015] In the same manner as discussed in Comparative Example A, catalysts listed in the following TABLE I were prepared. Each of these catalysts as well as Comparative Catalyst A was tested for Its catalytic activity in the ammoxidation of propylene to acrylonitrile. In carrying out this test, each of the catalysts was charged into a 5 cc. fixed-bed reactor. A feed of propylene/ammonia/oxygen/ nitrogen/steam in amounts of 1.8/2.2/3.6/2.4/6 was fed to the reactor such that the WWH was 0.1 g. propylene per gram catalyst per hour and the contact time was three seconds. The reaction temperature was maintained at 420°C. The results obtained as well as the results obtained when Comparative Catalyst A was employed was set forth in the following TABLE I.

    The parentheses used in TABLE I as well as the following TABLE II have no significance other than to clarify the difference between the various catalysts.

    Examples 8 to 10



    [0016] Using the various catalysts prepared in the manner described above, additional examples in which propylene was ammoxidized to acrylonitrile were conducted. These additional experiments were conducted in accordance with the same procedure used in Exanples 1 to 7, except that the reaction temperature was 430°C, the contact time was 6 seconds and the catalyst support was 505 SiO2. The results obtained are set forth in the following TABLE II.




    Claims

    1. Oxidation catalysts characterized by the general formula:

    wherein J is an alkali metal, thallium, silver or mixtures thereof;

    Q is Co, Ni, Zn, Cd, Be, Mg, Ca, Sr, Ba, Ra or mixtures thereof;

    Z is a two-or-more element system comprising Ge + Sb, Cu + W, Cu + Sn, Ce + W, Pr + Mn, Sn + Mn, Mn + W, W + Sb, Cr + Sn, W + Sn, Ge + Sn, Sb + Sn, W + P, Sb + P, Cr + Cu, Mn + Cu, Sb + Cu, Mn + P or mixtures thereof with the proviso that said catalyst is free of Tl when Z is Mn + P;

    D is Bi or Te; and

    wherein a is a number from 0 to 5;

    b is a number from 0 to 20;

    c is a number greater than 0 to 20;

    d is a number from 0 to 20;

    e is a number from 0 to 20; and

    x is a value such that the valence requirement of the elements in the catalyst for oxygen are satisfied;


    each element in said two or more element system being present in an amount of at least 1 atom percent based on the atoms in the system.
     
    2. The catalysts of claim 1 characterized in that

    a is a number from 0.01 to 0.5;

    b is a number from 0.1 to 20;

    c is a number from 0.1 to 9;

    d is a number from 0.1 to 20; and

    e is a number from 0.1 to 20.


     
    3. The catalysts of claim 2 characterized in that D is Bi.
     
    4. The catalysts of claim 3 characterized in that Z is either Ge + Sb, Cu + W, Cu + Sn, Ce + W, Pr + Mn, W + Sb, Cr + Sn, W + Sn, Ge + Sn, Sb + Sn, W + P, Sb + P, Cr + Cu, Mn + Cu, Sb + Cu, Mn + P, Sn + Mn or Mn + W.
     
    5. The catalysts of claim 3 characterized in that said catalysts contain at least one of K, Rb, and Cs and at least one of Co and Ni.
     
    6. Process for the preparation of acrylonitrile or methacrylonitrile by the reaction of propylene or isobutylene, molecular oxygen and ammonia at a temperature of about 200°C to 600°C in the presence of a catalyst, characterized in that a catalyst according to any of claims 1 to 5 is used.
     





    Search report