[0001] This invention relates to a process and apparatus for the manufacture of fibrils.
[0002] The Parrish patent U. S. 2, 988, 782 discloses the manufacture of very fine polymer
filaments that can be employed to manufacture water- laid sheets of synthetic paper.
These synthetic filaments are of such a small diameter that they behave quite differently
from spun filaments and have been characterized in the art as "fibrils" or "fibrids".
[0003] The Parrish process for preparing such fibrils involves preparing a solution of a
polymer in a suitable solvent and adding the polymer solution to a vigorously-agitated
solution of a liquid, which is a nonsolvent for the polymer of interest. As the polymer
solution is added to the vigorously-stirred nonsolvent liquid, the droplets of the
polymer solution are subjected to sheer forces and attenuated while simultaneously
being precipitated. Parrish discloses that the precipitation step is carried out in
a high intensity mixer such as a Waring blender, While the Parrish process is suitable
for making small laboratory quantities of such fibrils, the process is not well suited
to make substantial quantities of the fibrils at an acceptable cost.
[0004] The Davis, et al, patent U. S. 4, 013, 751 discloses an alternate process for preparing
fibrils by modified methods in which a hot polymer solution is passed through a hammermill
and suds cooled as the streams of polymer solution are thrown free of the rotating
plate of the hammermill. While this process provides; good quality fibrils, the process
is capital intensive and has higher manufacturing costs than is desired.
[0005] There is a need in the art for improved apparatus and processes for manufacturing
fibrils at a lower cost.
[0006] Novel centrifugal spinning apparatus has been developed for the manufacture of fibrils
from hot viscous hydrocarbon solutions of olefin polymers having an inherent viscosity
of at least 3. 5. The apparatus consists of an impeller which rotates at high speed
in a cylindrical cavity having a discharge port. The impeller has a plurality of blades
whose narrow dimensions lie substantially in the plane of the impeller's rotation
and whose tips come in close proximity to the inner peripheral surface of the cylindrical
cavity. The blades are arranged in at least two substantially-identical sets. Within
each set, the blades are offset substantially equidistant from one another; both in
the rotational plane of the impeller and in the plane transverse thereto. Two inlet
ports are provided in the peripheral surface of the cylindrical cavity to feed hot
polymer solution and coolant liquid to the cylindrical cavity, each of which port
is narrow in a plane transverse to the plane of the impeller's rotation and extends
over substantially the entire peripheral surface. The inlet ports are positioned near
the discharge port of the cylindrical cavity and upstream thereof viewed with respect
to the impeller's rotation, so that the bulk of the liquids entering the cavity from
the inlet ports are swept away from the discharge port by the impeller's rotation.
[0007] The hot polymer solution fed to the appratus is broken up into droplets by the rotating
impeller blades. Individual droplets impinge upon the surface of the impeller blades
and are attenuated into thin streams. In a like manner, the coolant liquid impinges
upon the impeller blades and cools the attenuated polymer streams to precipitate the
solute polymer in the form of fibrils.
Fig. 1 is an end view of one embodiment of centrifugal spinning apparatus of the invention,
partially in section, with parts broken away.
Fig. 2 is a view taken through lines 2-2 of Fig. 1.
Fig. 3 is a view of the rotating impeller blades as seen from the inner peripheral
surface of the apparatus of Fig. 1 with the peripheral surface extended into a flat
plane to show the pattern made by the rotating blades.
Fig. 4 is a view taken through lines 4-4 of Fig. 3.
Fig. 5 is a side plan view showing three pieces of the centrifugal spinning apparatus
shown in Fig. 1 ganged together and driven by a common shaft.
[0008] Referring to Fig 1 and 2, the centrifugal spinning apparatus includes a housing 20
having a cavity 30 machined therein and having a downwardly and outwardly extending
lower discharge port 22 which terminates at its lowermost end in an opening 24. The
ratio of diameter to depth in cavity 30 preferably is at least 5.0:1.0. Cavity 30
normally is covered and sealed by a removable front plate 32,Front plate 32 is held
in position on the front of housing 20 by means of a plurality of nuts 34 secured
to the ends of bolts 36 which are pivotally mounted to housing 20 and extend through
U-shaped slots 38. An impeller is mounted within cavity 30 on shaft 40 and consists
of four blades 42, 44, 46 and 48. The impeller blades are separated from each other
by washers not shown and are locked in fixed positions by suitable keys not shown.
The two halves of each blade are shown as, respectively, 42a and 42b, 44a and 44b,
46a and 46b, and 48a and 48b. The blades are offset from each other in fixed positions
so that the blades 42a, 44a, 46a and 48a constitute one set of blades, each of which
is offset substantially equidistant from each other, both in the rotational. plane
of the impeller and in the plane transverse thereto. In a like manner, the blades
42b, 44b, 46b and 48b constitute a second substantially-identical set of blades, with
these blades also being offset substantially equidistant from each other, both in
the rotational plane of the impeller and in the plane transverse thereto. The impeller
rotates in the direction of the arrow at high speed so that the tip speed of each
of the blades is at least about 200 feet per second and preferably greater than 500
feet per second.
[0009] Two inlet ports 50 and 52 of rectangular cross section are provided in the inner
peripheral surface of cavity 30, and extend over substantially the entire inner peripheral
surface in a plane transverse to the rotational plane of the impeller. Tapped openings
in the peripheral surface communicate with inlet ports 50 and 52 and are, threaded
to receive liquid feed tubes 54 and 56.
[0010] In operation of the process, it is customary to drive anore plurality of units from
a single shaft, Fig
. 5 illustrates three units being ganged together for operation off one drive shaft.
[0011] While the apparatus illustrated in the drawings represents the preferred embodiment
of the invention as presently perceived by the applicants, a number of modifications
can be made therein, The apparatus illustrated contains four impeller blades which
constitute two separate sets of blades. By increasing the ratio of the cylindrical
cavity's depth to its diameter, it is possible to mount a significantly greater number
of blades on the shaft. While the illustrated apparatus is mounted so that the impeller
blades rotate in the earth's gravitational field, the apparatus can be rotated 90°
so that the impeller rotates in a plane perpendicular to the earth's gravitational
field. When operated in this mode, the product discharge port is in one side of the
apparatus and the centrifugal force of the impeller blades transfers product into
the discharge port.
[0012] In operation the impeller is rotated by an external motor at high speed to provide
tip speeds in excess of 200 ft. /sec. At these speeds, the two tips of each blade,
e. g. 42a and 42b, 44a and 44b, etc. , function essentially as one continuous knife
blade. This action is shown in Fig. 3 in which rotation of the impeller blades is
shown in an extended, flattened plane. A polymer solution, consisting of about 4 weight
% of a high molecular weight olefin polymer having an intrinsic viscosity of at least
3.5 dissolved in a kerosene-type hydrocarbon, heated to a temperature of about 190°C,
is fed to cavity 30 through inlet port 50. Upon entering cavitty 30, the polymer solution
impinges upon the impeller blades and is broken up into a multiplicity of droplets
which are carried by centrifugal forces around the periphery of cavity 30 until they
reach discharge port 22. Virtually all of the droplets of polymer solution will come
into contact with the face of an impeller blade. When this occurs the droplets as
indicated by 60 and 62 in Fig 4 are attenuated by centrifugal force to form thin polymer
streams as shown, this action having the effect of orienting the solute polymer molecules
in the direction of the applied centrifugal force.
[0013] A coolant liquid, preferably water, is fed to cavity 30 through inlet port 52. The
coolant liquid impinges upon the impeller blades and is carried to discharge port
22 by centrifugal forces in the manner previously described. Upon contacting the impeller
blades, the coolant liquid removes heat from the blades which cools the polymer solution
in contact therewith and causes the polymer to precipitate from the solution in the
form of fibrils.
[0014] When the polymer solution, precipitated fibrils and coolant liquid come to the discharge
port 22, they leave the centrifugal spinning apparatus via opening 24 and are collected
for further processing and recovery, Typically, the product will be treated and recovered
in the manner as illustrated and discussed in U.S. 4, 013, 751. Specifically, the
product will be passed through a wringer to express the bulk of the liquid from the
polymer solids which then wil be beat one or more times in isopropanol to remove the
remainder of the solvent and coolant liquid from the fibrils. The fibrils then are
filtered and dried for use.
[0015] The process of the invention can be employed to prepare fibrils from essentially
any polymer solution in which the difference in polymer solubility between the two
operating temperatures is sufficient large. The quality of the fibrils produced, of
course, will be importa influenced by the polymer from which they are prepared.
[0016] Fibrils of optimum properties are prepared from olefin polymers having a very high
molecular weight such that the polymer has an intrinsic viscosity of at least 3. 5.
One species of such polymers consists of ethylene polymers containing, on a weight
basis, at least 9 0% of polymerized ethylene. Such ethylene polymers will be ethylene
homopolymers or ethylene copolymers containing small quantities of C
4 or higher olefin comonomer such as butene, hexene, styrene, a conjugated diene such
as butadiene, or the like. A second species of such olefin polymers consists of propylene
polymers containing, on a weight basis, at least 50% of polymerized propylene. Such
propylene polymers will be propylene homopolymers, or propylene copolymers containing
up to 50% of copolymerized ethylene.
[0017] In the preparation of the fibrils of this invention, fibrils having a highly satisfactory
combination of overall properties are obtained when the polymer employed in the process
consists entirely of an olefin polymer as described above. It has been observed, however,
that fibrils of generally satisfactory properties can be cb tained when a mixture
of polymers is employed in the process, provided that the olefin polymer as described
above, constitutes at least about 20 weight % and preferably at least 35 weight %
of the total polymer employed in the fibril-manufacturing process.
[0018] Where polymers other than an olefin polymer, as described above, are employed as
a part of the polymer used in the fibril-manufacturing process, the other polymers
employed may be employed for either of two principal purposes. For one, such other
polymers can be employed principally to lower the raw material cost of the fibrils
to be prepared. In some cases, such other polymers can be employed to modify specific
properties of the fibrils themselves, or the water-laid, paper-like sheets prepared
therefrom. Regardless of the purpose for which such other polymers are employed, for
convenience of description, the polymers employed in the fibril-manufacturing process,
in addition to the olefin polymers described above, will be referred to as "diluent
polymers". Diluent polymers suitable for this purpose are those set forth in U. S.
4, 013, 751.
[0019] The solvent to be employed in the process of the invention may be any liquid which
will completely dissolve the olefin polymer employed in the process at an elevated
temperature. It is highly desirable that the solvent employed have a significantly
different capacity to dissolve the olefin polymer at different temperatures. The ideal
solvents are those having a very low solubility for the olefin polymer at ambient
temperature, but having a high degree of solvent power for the olefin polymer at temperatures
above 140 C. Hydrocarbon solvents such as kerosene, mineral spirits, tetraline and
aromatic hydrocarbons such as xylenes, have excellent characteristics for use in the
invention and are the preferred solvents to be employed in the invention. Other solvents,
however, such as certain of the chlorinated hydrocarbons, also can be employed if
desired. The solvents employed should be liquids at ambient temperature and preferably
should have atmosphe boiling points above 150°C and preferably above 180 C .
[0020] The polymer solutions employed in the process should be heated to temperatures of
at least 100°C and preferably 150°C or higher. Polymer concentrations of 2 weight
% or higher should be employed.
[0021] By reason of the process by which the fibrils of the invention are prepared, it is
possible to make many modifications of the fibrits which improve their utility in
the manufacture of waterlaid sheets. By way of example, certain inorganic pigments,
fillers, and the like can be incorporated into the polymer solution and remain physically
encapsulated within the polymer filaments when they are precipitated from the fine
polymer streams in the cooling step. Typical of the pigments that can be employed
for this purpose include titanium dioxide, silica, calcium carbonate, calcium sulfate,
and the like. In another variation of the invention, cellulosic papermaking fibres
can be incorporated into the polymer solution and are encapsulated within the monofilaments
in the cooling step. Waterlaid sheets prepared from such modified fibrils have enhanced
opacity, improved printing characteristics, high water resistance, and the like
1. Apparatus for the manufacture of polymer fibrils from a hot viscous solution of
thermoplastic polymer consisting essentially of:
a, a housing having a cylindrical cavity therein
b. an impeller mounted for rotation within said cylindrical cavity, said impeller
having a plurality of blades whose narrow dimensions lie substantially in the plane
of the impeller's rotation and whose tips come in close proximity to the inner peripheral
surface of the cylindrical cavity.
c. a discharge port in the bottom of said cylindrical cavity.
d. first and second liquid inlet ports in the peripheral surface of the cylindrical
cavity, each of said ports being narrow in the plane transverse to the plane of the
impeller's rotation and extending over substantially the entire peripheral surface.
e. said liquid inlet ports being positioned so that they are near the discharge port
of the cylindrical cavity and upstream thereof viewed with respect to the impeller's
rotation, so that liquids entering said inlet ports are swept away from the discharge
port by rotation of the impeller, and
f. means for feeding different liquids to the first and second inlet ports.
2. Apparatus of claim 1 in which the narrow dimension of the impeller's blades is
less than about one inch, in which the blades are arranged in at least two substantially-identical
sets and in which, within each set, the blades are offset substantially equidistant
from one another, both in the rotational plane of the impeller and in the plane transverse
thereto.
3. Apparatus of claim 2 in which the ratio of the cylindrical cavity's diameter to
its depth is at least about 5.0:1.0.
4. Apparatus for the manufacture of polymer fibrils from a hot viscous solution of
thermoplastic polymer consisting essentially of;
a, a housing having a cylindrical cavity therein
b. a discharge port in said housing.
c. means for feeding two different liquids into said cylindrical cavity,
d. an impeller which rotates within said cylindrical cavity at a speed to provide
blade tip speeds of at least about 200 ft/sec.
e. the blades of said impeller having their narrow dimension in their plane of rotation,
and
f. the tip of said impeller blades rotating in close proximity to the inner peripheral
surface of said cylindrical cavity.
5. Apparatus of claim 4 in which the narrow dimension of the impeller's blades is
less than about one inch, in which the blades are arranged in at least two substantially-identical
sets and in which, within each set, the blades are offset substantially equidistant
from one another, both in the rotational plane of the impeller and in the plane transverse
thereto.
6. A process for preparing fibrils from a hot viscous solution of a thermoplastic
polymer which consists essentially of:
a. rotating an impeller at high speed in a cylindrical cavity, said impeller having
a plurality of blades whose tips come in close proximity to the inner peripheral surface
of said cylindrical cavity, the blades of said impeller having their.narrow dimension
substantially in the plane of impeller rotation
b. feeding a stream of a hot viscous solution of thermoplastic polymer into said cylindrical
cavity to impinge upon the blades of said impeller near their tips so that said polymer
solution contacts said blades, is broken up into droplets and/or thin streams which
flow over the surfaces of said blades whereby the polymer solution is subjected to
high sheer stresses and attenuated to orient the solute polymer molecule in said polymer
solution,
c. feeding a stream of coolant liquid into said cylindrical cavity to impinge upon
the blades of said impeller near their tips so that said coolant liquid is broken
up into droplets and/or thin streams which flow over the surfaces of said blades,
and cool the polymer solution in contact therewith to precipitate fibrils therefrom,
and
d. withdrawing a stream of fibrils, polymer solvent, and coolant liquid from the cylindrical
cavity.
7. A process of claim 6 in which the polymer solution fed to the process is at a temperature
above 100°C, has a viscosity in excess of about 50 centipoises, and is a hydrocarbon
solution of a polymer selected from the group consisting of:
a, an olefin polymer having an intrinsic viscosity of at least 3. 5 and selected from
the group consisting of:
(i) an ethylene homopolymer,
(ii) a copolymer containing at least 90 weight percent of polymerized ethylene and
the balance a polymerized olefin hydrocarbon containing at least 4 carbon atoms,
(iii) a propylene homopolymer, and
(iv) a copolymer containing at least 50 weight percent of polymerized propylene and
the balance polymerized ethylene:
b. a mixture of olefin polymers of (a), and
c. a mixture of polymers containing at least 20 weight % of an olefin polymer of (a)
and up to 80 weight % of a diluent polymer that is soluble at 100°C in the solvent
employed in the process.
8. The process of claim 7 in which the coolant liquid is water.