[0001] The invention relates to a process for preparing copolymers by polymerization in
aqueous dispersion of 25-85 parts by weight of styrene and/or a-methyl styrene with
75-15 parts by weight of acrylonitrile and/or methacrylonitrile and, possibly, minor
quantitites of one or more other monomers, optionally in the presence of a rubber,
with the aid of one or more compounds yielding free radicals, in which process an
additional amount of a compound yielding free radicals is added after the conversion
has reached a value of more than 75 w.-%.
[0002] This process is well-known and is applied on a large scale in industry. However,
it yields products that may contain a considerable quantity of non-converted monomers.
[0003] This quantity may even lie in the order of magnitude of a few per cent, depending
on the polymerization conditions. The monomer residues are highly undesirable. They
have an adverse influence on the properties of the end product, such as gloss and
heat resistance, and may moreover be released from the product during its subsequent
processing or in its application, which is highly undesirable in view of the negative
environmental impact and the toxicity.
[0004] Therefore, intensive research has been carried out for a long time already to find
methods to reduce the monomer content of such polymers. It has been proposed to treat
the polymer dispersion with steam for the purpose of stripping part of the non-converted
monomers from the polymer. This treatment may be effective, particularly with protracted
treating, but it is expensive, as regards investment as well as energy consumption.
[0005] It has also been proposed to carry out the removal of monomers in a so-called degasifying
extruder. To this end, the polymer is melted in an extruder with simultaneous build-up
of a high pressure.
[0006] Next, the product comes in a zone where the pressure has been strongly reduced and
where the volatile components are exhausted. This process requires very high investments,
especially because the capacity of this degasifying extruder is, of necessity, low
if a high removal efficiency is to be achieved. In U.S. Patent Specification 3.991.136
it has been proposed that, after the polymerization has proceeded to a degree of conversion
of 90%, a new monomer be added which is very reactive with the non-converted monomer.
This new monomer should be added in a quantity of 5 to 10 w.-%, so that it will have
a substantial influence on the polymer properties. Further, an additional monomer
involves relatively high cost because of the extra investments and operations its
requires.
[0007] The purpose of the invention is providing a process which yields polymers of a very
low monomer content, without monomers of another kind having to be applied. Another
purpose of the invention is providing a solution to the problem of removing non-converted
monomer without negatively influencing the properties of the polymer. A further purpose
of the invention is reducing the environmental impact and the possible risks from
monomer emission during the production and processing of the polymer. It is also a
purpose of the invention to raise the capacity of the polymerization reactors. Further,
it is a purpose of the invention to utilize the monomers applied in a more efficient
way.
[0008] It has now been found that these purposes can be fulfilled by adding to the polymer
dispersion, at a carefully chosen point of time, a certain amount of a special compound
yielding free radicals.
[0009] The process for preparing copolymers according to the invention is characterized
in that a compound which yields water-soluble free radicals which can be the same
as, or different from the compound used at the beginning of the polymerization is
additionally supplied in a quantity of 0.05-2.5 parts by weight per 100 parts by weight
of total monomer after the conversion rate has become smaller than 15 w.% per hour,
and the addition of monomers has been terminated, while at least 0.1 w.-% of non-converted
(meth)acrylonitrile remains in the reaction medium.
[0010] The weight percentage of non-converted (meth)acrylonitrile is calculated with reference
to the total reaction medium, i.e. water together with substances dissolved and dispersed
in it.
[0011] It is to be considered as highly surprising that a simple measure as described above,
provided it is carried out at the correct point of time and with the proper compounds,
is capable of drastically reducing the monomer content, without affecting the properties
of the polymer, of increasing at the same time, not insubstantially, the capacity
of the polymerization reactor employed and, also, of causing the monomer feedstocks
supplied to be used more efficiently.
[0012] Even, the properties of the polymer are improved by employing this measure. For it
has been found that the flow and the heat distortion temperature are improved when
using the process according to the invention. Moreover, the process according to the
invention leads to substantial reduction of the drying-time of certain products.
[0013] One should expect that the addition of an extra amount of a compound yielding free
radicals yields a copolymer whose composition deviates from the polymer already prepared,resulting
in inhomogeneities. In particular, it would be expected that at the end of the polymerization,
when the polymer to monomer ratio is very high, transfer reactions with the polymer
would occur, which may result in linkage reactions which affect the processability
(see Emulsion Polymerization Theory & Practice, D.C. Blackley, 1975, pp 71 and 72).
It appears that these disadvantages do not occur if one proceeds according to the
present invention.
[0014] It was found that the effect of the present invention cannot be reached through an
increase in the quantity of initiator which is added at the beginning or in the course
of the polymerization, but before the moment specified according to the invention.
[0015] It is of great importance that the extra addition of initiator is not effected too
early, but not too late either. The quantity of non-converted (meth)acrylonitrile
in the reaction medium should be at least 0.1 w.-%. Preferably, this weight percentage
should be at least 0.2 w.-% or, specifically, at least 0.5 w.-%. At lower values,
no or hardly any reduction of the proportion of residual monomers occurs, especially
as regards the proportion of styrene and a-methyl styrene. This is very surprising
as styrene in particular is known to polymerize very easily.
[0016] In general, polymerizations in dispersion show a maximum in the conversion rate,
which maximum expresses itself in the form of a temperature peak that cannot be fully
coped with by cooling. Supply of compounds yielding free radicals at about the point
of time this temperature peak occurs proves not to produce the required, favourable
result. On the contrary, the result is even negative in relation to a number of properties
like the notch impact strength at low temperature and the stiffness, so that such
supply, therefore, should be considered a pure waste of auxiliary material(s). The
process according to the invention is the more surprising as the field of polymerization
of monomers in aqueous dispersion as for a long time already been the subject of much
research. Since these polymers are moreover produced and applied in very large quantities,
the results of the present invention are of very great importance.
[0017] The polymerization according to the invention takes place in an aqueous dispersion.
The term aqueous dispersion is understood to include both emulsions and suspensions.
The present invention is aimed in particular at the emulsion polymerization because
in this polymerization the best results are obtained.
[0018] The extra monomers of which one or more may be included in the polymerization process
in minor proportions are, among other, ionogenic vinyl compound and/or alkyl compounds,
flame killers to be built in, or multi-functional compounds, such as di-vinyl benzene
or an alkyl ester of (meth)acrylic acid. Special preference is given to polymers which
contain more than 50 w.-% of styrene, in particular a-methyl styrene.
[0019] Especially in the case of a-methyl styrene polymers the greatest problems occur in
relation to the monomer content in the finished product.
[0020] a-Methyl styrene monomer is very difficult to remove then. Particularly with these
polymers the present invention appears to yield excellent results.
[0021] The emulsion polymerization can be carried out with a good result in the presence
of a previously prepared rubber latex, for instance, a polybutadiene latex. In addition
to the free polymer formed also a graft polymer may form, which is of importance to
the impact strength.
[0022] In the polymerization in aqueous dispersion the usual auxiliary materials necessary
for that purpose should be applied, such as emulsifiers, lye, suspension agents, salts,
soaps, initiators like peroxides, and molar-weight regulators. In the emulsion polymerization
one chooses preferably alkali-or ammonium-persalts and/or redox systems for initiators.
In particular, mention is to be made of potassium persulphate, ammonium persulphate
and sodium persulphate. Examples of redox systems are persalts, (e.g. perchlorates
or persulphates), tert. butyl hydroperoxide, cumene hydroperoxide, diisopropyl benzene
hydroperoxide and methyl cyclohexyl hydroperoxide, combined with reduction agents
based on acids containing sulphur in a low-valency state, such as sodium formaldehyde
sulphoxylate, bisulphite, pyrosulphite, or with organic bases (like triethanolamine),
with dextrose, sodium pyrophosphate and mercaptans or combinations thereof, optionally
in combination with metal. salts such as ferrous sulphate. These initiators or initiator
systems may be supplied all at once, stepwise or even gradually.
[0023] Generally, the polymerization in emulsion starts only slowly. The conversion rate
increases slowly, to reach a few hundred per cent per hour at the highest value. This
means a considerable heat production within a relatively short time, which results
in a temperature increase because the cooling cannot cope with this rapid heat development.
Subsequently, the conversion rate will decrease slowly, whereupon according to the
state of the art, the polymerization is discontinued at a point of time at which the
polymerization rate has become too small for the polymerization still to be continued
to advantage.
[0024] However, according to the present invention, after the conversion degree has reached
a value of more than 75% by weight and the conversion rate has become lower than 15%
by weight per hour and after the monomer addition has been terminated, while at least
0.1 wt.-% of non-converted (meth)acrylonitrile) remains in the total reaction medium,
a compound yielding water-soluble free radicals is added additionally. In this way
it is achieved that the total polymerization time is not extended. This yields the
great advantage of an increased production capacity of the polymerization reactor
without any appreciable investments.
[0025] At the same time, a polymer is obtained having such a low monomer content that the
capacity problems occurring in the subsequent processing to, for instance, granulate,
are eliminated straight away. These capacity problems are the results of the measures
to be taken to decrease the high monomer content, namely intensive and long drying
and/or the application of degasifying extruders. The compounds yielding water-soluble
free radicals are, themselves, often completely water-soluble. Examples are persulphates,
such as potassium persulphate and ammonium persulphate. But also compounds which are
not completely water-soluble but yield water-soluble free radicals can be applied
with very good results. Examples are the tert.-butyl-peroxy compounds, like di-tert.
butyl peroxide, di-tert. butylperoxydicarbonate, tert. butyl peracetate, tert. butyl
perpivalate, tert. butyl perbenzoate, and tert- butyl hydroperoxide. These compounds
are particularly preferable because very stable latices are obtained. This is of importance
during transportation and storage of the latices. Further, also compounds which are
not completely water-soluble and which form part of a redox system that yields water-soluble
free radicals can be applied.
[0026] Examples of compounds of this kind are hydroperoxides, such as cumene hydroperoxide,
diisopropyl benzene hydroperoxide, triisopropyl benzene hydroperoxide, tert. butyl
isopropyl benzene hydroperoxide and dodecyl isopropyl benzene hydroperoxide.
[0027] The amount of additionally added compound yielding free radicals preferably amounts
to 25 to 500% by weight, particularly to 50 to 300%, by weight of the quantity of
initiator added previously. Although in itself not necessary, it may offer advantages
if the additionally supplied initiator consists of the same compound which was supplied
at the beginning of the polymerization.
[0028] The additionally added compound yielding free radicals is preferably added after
the conversion degree has become larger than 80%, by weight in particular larger than
90% by weight. Conversion degree is understood to mean the quotient of the quantity
of monomers converted into polymer and the total quantity of added monomers, multiplied
by 100%. The addition does not take place until the conversion rate has become very
low i.e. less than 15% by weight per hour, by preference lower than 8% by weight per
hour, more particularly lower than 4% by weight per hour.
[0029] At the time the additional amount of compound yielding free radicals is added, the
temperature should be sufficiently high. Preference is given to temperatures above
30°C, preferably above 45°C. But the temperature should not be chosen too high. Suitable
temperatures lie below 120°C, in particular below 100°C. The half-life period of the
compound yielding free radicals at these temperatures is, by preference, not too high,
i.e. smaller than 5 hours, in particular smaller than 2 hours. It is advantageous
to apply short half-life periods, which can be done by the choice of the temperature
and/or the compound yielding free radicals. A half-life period smaller than 1 hour
is the most preferable.
[0030] In the following examples all percentages are given by weight, unless otherwise indicated.
Example I
[0031] 52g of acrylonitrile, 20g of styrene and 98g of a-methyl styrene were added, with
exclusion of air, to 420 g of oxygen-free, deionized water, in which were dissolved
0.28 g of KOH and 4.0 g of rosin soap and an emulsion was formed having a temperature
of 75°C. After the reaction mixture had been brought to 50°C, with an oil bath, a
redox initiator system was subsequently added to it which consisted of: 0.84 g of
cumene hydroperoxide, 0.02 g of ferrous sulphate dissolved in 10 g of water, and the
mixture of 1.0 g of sodium pyrophosphate in 1.2 g of dextrose dissolved in 30 g of
water.
[0032] Owing to the heat of polymerization, the temperature in the polymerization medium
rose in 31 minutes to 86.5°C and dropped thereupon gradually to 75°C. To determine
the content of non-converted monomer in the total reaction medium, a sample of 1 ml
was taken from the reaction medium after 90 minutes, counting from the point of time
the initiator system was added, in which sample, after dilution with dimethyl formamide,
the quantity of non-converted monomer was determined gas-chromatographically, from
which the monomer conversion was calculated. This amounted to 94.9% at this point
of time. The polymerization rate can be determined by taking 2 samples in succession
with a known, short time interval. This rate amounted to 1.2% per hour at this point
of time. Immediately after the sampling, 0.34 ml of a 75% solution of tert. butyl
perpivalate in mineral oil was added to the reaction mixture in accordance with the
process of the invention. The half-life period of this peroxide amounts to 0.8 hr
at 75°C. Next, the residual monomer content in the reaction medium was determined
after 120 and 150 minutes from the beginning of the polymerization, in the same way
as described above. From the various concentrations after 90 and 150 minutes the monomer
conversion during the last hour of the polymerization can be calculated, viz.

The results are mentioned in table 1, under No. I.
Comparative example 1 A
[0033] The realization of this polymerization is completely identical with that described
in example I, on the understanding that addition of tert. butyl perpivalate was omitted
in this experiment.
[0034] Comparing the residual monomer contents of this comparative example with those of
example I clearly shows that the decrease of the acrylonitrile- and the styrene- and
the α-methyl styrene monomer concentration is considerably greater in the process
according to the invention than in the comparative example (see table 1, experiment
I A).
Example II
[0035] Example I was repeated, 60 g of a polybutadiene rubber latex containing 50 w.-% of
solid being added to increase the impact strength, whilst the total quantity of water
of example I was kept constant.
[0036] The results can be found in table 1.
Comparative. example II A
[0037] In order to demonstrate additionally the effect of the extra supply of the compound
yielding free radicals according to the invention also in the presence of rubber,
example II was repeated, but without addition of tert. butyl perpivalate. This experiment
was carried out in duplicate; the results thereof are given, between parentheses,
in table 1.
Comparative example II B
[0038] In order to demonstrate that the addition of the extra supply of compound yielding
free radicals must take place after the conversion has become larger than 75% the
experiment of example II was repeated, the tert. butyl perpivalate being added at
the peak temperature, at which point of time the conversion amounted to 72% according
to gas-chromatographic analysis. The conversion rate amounted to 83%/hr at this moment.
The results show that in the last part of the polymerization no extra decrease of
the free monomer content is obtained (see table 1).

Example III
[0039] In this example the polymerization of acrylonitrile, styrene and a-methyl styrene
was carried out in 2 steps, in which, according to the invention, extra potassium
persulphate was added at the end of the second step. In the first step, successively,
the following were added to a polymerization vessel, while stirring: 230 g of water,
60 g of a 50% polybutadienelatex, 2 g of rosin soap, 0.14 g of KOH, 10 g of styrene,
26 g of acrylonitrile, 49 g of a-methyl styrene, and 0.2 g of tert. dodecyl mercaptan.
After this reaction mixture had been heated to 40°C with the aid of a bath of 65°C,
the initiator system was added, consisting of: 0.84 g of cumene hydroperoxide and
1.2 g of dextrose + 1.0 g of sodium pyrophosphate, dissolved together in 30 g of water,
and 0.02 g of ferrous sulphate dissolved in 10 g of water. After 2 hours about 95%
of the monomers had been converted into polymer. Subsequently, for the second step
of the polymerization, the following was added to the polymer latex formed: 150 g
of water, 2 g of rosin soap, 0.14 g of KOH, 10 g of styrene, 26 g of acrylontrile,
49 g of α-methyl styrene, and 0.6 g of tert. dodecyl mercaptan. After this mixture
had again reached a temperature of 50°C, 0.4 g of potassium persulphate dissolved
in 10 g of water was added to it as initiator. 90 minutes after the second step of
the polymerization had been started, the conversion, determined gas-chromatographically,
amounted to 90.5%. At this point of time, according to the invention, 0.4 g of potassium
persulphate dissolved in 10 g of water was added and the decrease of the non-converted
monomer was continued. For results, see table 2.
Comparative example IIIa
[0040] Example III was repeated, without application however, of the extra potassium persulphate
supply at the end of the second step. Comparison of the results of experiments III
and Illa shows that in the process according to the invention a substantially improved
monomer removal has taken place.

Examples IV to X incl.
[0041] In this series of examples, example I was repeated, a different initiator being added,
however, in each example after 90 min. In examples IV and V, forming part of the invention,
considerably more monomer was converted into polymer during the last hour of the polymerization
than in examples VI to X incl., in which a radical-yielding compound was applied which
generates water-insoluble radicals. For the results, reference is made to table 3.

Examples XI and XII
[0042] These examples were a repetition of example I. The polymerization process was applied
to a mixture containing acrylonitrile and a-methyl styrene, but no styrene, and instead
of the redox initiator system, potassium persulphate was used. After a polymerization
time of 120 minutes, 0.8 g KPS dissolved in 10 g water was added.
[0043] The composition of the monomer mixture was such that the concentration of the water-soluble
component (acrylonitrile) under these polymerization conditions varied strongly at
the time of adding the extra quantity of KPS.
[0044] From the calculated monomer conversion during the last hour (mon. conv.) it clearly
appears that α-methyl styrene removal decreases strongly as the ACN concentration
in the latex declines.
[0045] For results see table 4.
Comparative Example XIII
[0046] In this comparative example, which was analogous to examples XI and Xil, the monomer
mixture was such that the acrylonitrile concentration in the latex at the time of
addition of the extra quantity of KPS was lower than 0.1%.
[0047] The results show that at this low ACN concentration the level of α-methyl styrene
removal was considerably lower than in examples XI and XII in spite of the extra addition
of initiator. The level of α-methyl styrene removal is about the same as reached without
extra addition of water-soluble initiator (also see comparative example I a).
[0048] For results see table 4.

Example XIV
[0049] In this example, a ternary mixture of acrylonitrile, a-methyl styrene and methacrylate
allyl ester in weight proportions of 31.9, 67.7 and 0.4, respectively, was polymerized
in emulsion, as described in example I, with potassium persulphate as initiator. One
hour before termination of the polymerization, 0.8 g potassium persulphate dissolved
in 10 g water was added. Upon termination of the polymerization, it appeared that
the monomer concentration in the latex was 0.22% for ACN and 0.13% for a-methyl styrene,
which means that the level of α-methyl styrene removal was very high.
Example XV
[0050] Example XIV was repeated with a ternary mixture containing 20.4 parts by weight of
acrylonitrile, 67.9 parts by weight of a-methyl styrene and 11.7 parts by weight of
methyl methacrylate (MMA). The MMA was not initially present, but was gradually supplied
to the reactor in about 40 minutes subsequent to addition of the initiator; 30% of
the required quantity of ACN was supplied to the reactor only after 190 minutes.
[0051] Next, after 240 minutes, 0.8 g potassium persulphate dissolved in 10 g water was
added.
[0052] After 300 minutes, it appeared that the monomer concentration in the latex was: ACN
+ MMA: 0.13% and α-m.s.: 0.63%.