(19)
(11) EP 0 000 720 B1

(12) EUROPEAN PATENT SPECIFICATION

(45) Mention of the grant of the patent:
07.07.1982 Bulletin 1982/27

(21) Application number: 78100474.2

(22) Date of filing: 21.07.1978
(51) International Patent Classification (IPC)3: C30B 17/00, C30B 29/28

(54)

Process for producing single crystal of yttrium-iron garnet solid solution

Verfahren zur Herstellung eines Einkristalls, der aus einer festen Lösung von Yttrium-Eisen Granaten besteht

Procédé de fabrication d'un monocristal d'une solution solide de grenat de fer et d'yttrium


(84) Designated Contracting States:
DE FR GB NL

(30) Priority: 09.08.1977 JP 95416/77
09.08.1977 JP 95417/77

(43) Date of publication of application:
21.02.1979 Bulletin 1979/04

(71) Applicant: NATIONAL INSTITUTE FOR RESEARCHES IN INORGANIC MATERIALS
Ibaraki, 300-31 (JP)

(72) Inventors:
  • Kimura, Shigeyuki
    Ibaraki-ken (JP)
  • Shindo, Isamu
    Ibaraki-ken (JP)
  • Mori, Yasumichi
    Ibaraki-ken (JP)
  • Kitamura, Kenji
    Tsuchiura-shi Ibaraki-ken (JP)
  • Ii, Nobuo
    Ibaraki-ken (JP)

(74) Representative: Wächtershäuser, Günter, Prof. Dr. 
Patentanwalt, Tal 29
80331 München
80331 München (DE)


(56) References cited: : 
   
       
    Note: Within nine months from the publication of the mention of the grant of the European patent, any person may give notice to the European Patent Office of opposition to the European patent granted. Notice of opposition shall be filed in a written reasoned statement. It shall not be deemed to have been filed until the opposition fee has been paid. (Art. 99(1) European Patent Convention).


    Description

    Background of the invention



    [0001] The present invention relates to a process for preparing a single crystal of an yttrium-iron garnet solid solution of the composition R3M5O12, wherein R represents Y which may be partly substituted by other rare earth elements and M represents Fe (III) which may be partly substituted by AI and/or Ga with the exception of Y3Fe5O12, at a single crystal growth rate of greater than 0.1 mm/h.

    [0002] Such a process is known from US patent 3444084. However, the prior art process is inflicted with a low growth rate and an insufficient purity of the obtained single crystals. These problems are increased if the number of the components is increased, notably if a quarternary solid solution is prepared. In case of such quarternary or higher iron garnet solid solutions considerable problems concerning a uniform distribution of the components arise.

    [0003] The Journal of Applied Physics, 32, 376S-377S (1961) teaches specific process conditions for obtaining a ternary yttrium-iron garnet solid solution. However, the process conditions for obtaining high-quality quarternary or higher yttrium-iron garnet solid solutions are not known from this publication. Therefore the present invention is concerned with the problem to prepare quarternary or higher yttrium-iron garnet solid solutions with a high purity and a uniform distribution of the components in spite of a high growth rate of the process.

    [0004] This problem is solved by a process which is characterized in that the floating zone method is used, whereby between an upper downwardly fed rotating rod of a mixture for the product and a lower downwardly moved counter rotating seed a solvent zone is maintained by radiation convergence heating under an oxygen pressure of at least 1.01 × 10-2 bar (at least 10-2 atm), whereby the composition of the solvent differs from that of the rod and is defined by a molar ratio of the M-component to the R-component of from 1:0.1 to 1:0.3 and in the presence of AI and/or Ga by a ratio of

    :n the range of 1:1.5 to 1:2.5, wherein x represents Al2O3 and/or G8203 and wherein M6 and MC symbolize the molar concentration in the solvent and in the solid solution, respectively.

    Detailed description of the preferred embodiments



    [0005] In the production of the single crystal of a yttrium-iron garnet solid solution, the solvent is contacted with the lower edge of the rod of the mixture for the product and the seed is contacted with the bottom of the solvent and the solvent part is heated to melt it by the floating zone method to form the single crystal of the product of R3M5O12 wherein R represents Y and optionally other rare earth element and M represents Fe and optionally AI or Ga.

    [0006] The rod of the mixture for the product comprises the yttrium oxide type component and the iron oxide type component at molar ratio of 2.5:5.0 to 3.5:5.0 wherein the yttrium oxide type component comprises Y203 as main component and optionally the other rare earth oxides as additional component, and the iron oxide type component comprises Fe203 as main component and optionally Al2O3 or Ga203 as additional component.

    [0007] The solvent comprises the iron oxide type component and optionally less than 0.6 mole of the rare earth oxide component per 1 mole of the iron oxide type component.

    [0008] The single crystal of the yttrium-iron garnet having the formula

    has a width of ferro-magnetic resonance absorption (AH) of less than 2 Oe under the alternating field of 9,300 MHz as a spherical ball having a diameter of 1 mm.

    [0009] The single crystal having higher quality can be obtained by recrystallizing the resulting single crystal of R3M5O12.

    [0010] The yttrium oxide and the other rare earth oxides can be the commercially available ones without any chemical treatment and preferably with a smaller diameter so as to promote the reaction with ferric oxide, aluminum oxide or gallium oxide; such as less than 1 mm especially, less than 10 µm.

    [0011] The purity of yttrium oxide and the other rare earth oxide can be of special grade. When the single crystal is used as a magnetic material, the contamination with impurity is remarkably disadvantageous whereby higher purities of the raw materials are preferable.

    [0012] It is further preferable for performing the reaction to use the raw material obtained by calcining it in air at high temperature e.g. 1000°C for a long time e.g. 1 day.

    [0013] The ferric oxide used in the present invention, can be in special grade and preferably has a small diameter so as to promote the reaction with the rare earth oxide, aluminum oxide or gallium oxide, such as less than 1 mm especially, less than 10 µm.

    [0014] The aluminum oxide used in the present invention, can be in special grade and preferably has a small diameter so as to promote the reaction with the rare earth oxide, ferric oxide or gallium oxide, such as less than 1 mm especially, less than 10 µm.

    [0015] The gallium oxide used in the present invention, can be in special grade and preferably has a small diameter so as to promote the reaction with the rare earth oxide, ferric oxide or aluminum oxide, such as less than 1 mm especially less than 10 µm.

    [0016] In the mixing operation, it is preferable to uniformly mix the raw materials. The mixing operation can be made by various methods such as a method of mixing them with an organic liquid such as alcohols and acetone in a mortar; a method of mixing them in a mixer such as a ball mill or a method of coprecipitation after dissolving them in an acid etc.

    [0017] The average diameter of powders of the mixture is preferably less than 1 mm especially less than 10 µm.

    [0018] The composition for the product of R2M5O12 used in the present invention is preferably a molar ratio of 2.5:5.0 to 3.5:5.0 of the rare earth oxide to the total of ferric oxide, aluminum oxide and gallium oxide. The ferric oxide is usually used as the main component for the iron oxide type component and a part can be substituted with aluminum oxide. or gallium oxide (greater than 0.1 mole% especially greater than 1 mole %). The magnetic characteristics of the product can be varied by varying the content'of aluminum oxide or gallium oxide. The magnetic or electric characteristics of the product may be improved by adding a small amount of the component of Ca, Sr, Ba, Sc, Ti, V, Cr, Mn, Co, Ni, Cu, Zn, Si or Ge if necessary.

    [0019] The solvent used in the present invention is a liquid medium for dissolving the mixture for the product of R3M5O12 and forming the single crystal of R3M5O12 from it.

    [0020] In the process of the present invention, the solvent comprises ferric oxide. The other components of aluminum oxide, gallium oxide, the rare earth oxides can be incorporated. The molar ratio of the total of ferric oxide, aluminum oxide and gallium oxide to the rare earth oxide is 1:0.1 to 1:0.3. The melting point of the solvent should be lower than the decomposition temperature of the product of R3M5O12.

    [0021] The content of aluminum oxide or gallium oxide is dependent upon the composition of the solid solution of the yttrium-iron garnet.

    [0022] When the molar concentrations of Fe2O3, A1103 and Ga203 in the solvent are designated as

    and the molar concentrations of the components in the solid-solution are designated as

    the ratio of

    is in a range of 1:1.5 to 1:2.5 especially 1:1.8 to 1:2.2. It is preferable to have the same relationship between



    [0023] In the compressing molding of the mixture, it is possible to employ a molding method using a mold for one directional compressing method or two directional compressing method. However, in order to prevent the curve of the rod in the heating step, it is preferable to employ a rubber press method wherein the pressure is hydrostatically applied.

    [0024] The rubber press method means that the powdery mixture is charged in a rubber tube and both ends of the rubber tube are sealed and the rubber tube is compressed under high hydraulic pressure in a sealed hydraulic apparatus. The hydraulic pressure is usually higher than 500 Kg/cm2 preferably 1 to 2 metric ton/cm2. The hydraulic pressure is usually applied for longer than 5 seconds preferably 1 minute. The molded product prepared under lower pressure is easily cracked.

    [0025] The molded mixture can have any rod type shape as it is used in the floating zone method. It is especially preferable to use a cylindrical rod having a diameter of 1 mm to 10 cm and a length of 1 mm to 5 m preferably a diameter of 3 mm to 1 cm and a length of 5 mm to 30 cm.

    [0026] In the calcination of the molded mixture, it is possible to heat it while holding it in a suitable crucible in a horizontal furnace. However, it is preferable to heat it in a vertical furnace in a suspended condition so as to prevent a contamination with impurities and not to cause a curve in the calcination.

    [0027] The furnace is to maintain greater than 1.01 ×10-2 bar (10-2 atm.) of oxygen and to be stable at the maximum temperature of 1,650°C, and preferably to maintain greater than 1.01 bar (1 atm.) of oxygen.

    [0028] The temperature for calcining the molded mixture is dependent upon the kind of the rare earth oxide and the content of AI or Ga and the pressure of oxygen in the environment, and it is preferably at 1,500 to 1,750°C in the case of the mixture for the product and at 1,400 to 1,450°C in the case of the mixture for the solvent. It is especially preferable to use the maximum temperature at which no liquid is formed in the oxygen environment in the case of the mixture for the product of R3M5O12·

    [0029] The time for calcining the molded mixture is preferably longer and it is preferable to calcine the molded mixture to give a bulk density of greater than 80% of the true density.

    [0030] The oxygen pressure in the environment of the calcination is preferably higher so as to prevent a formation of ferrous oxide component in the product of R3MIO,, because the ferrous oxide component causes inferior magnetic characteristics. In order to prevent the incorporation of an inert gas in the form of bubbles in the calcined product, it is preferable to prevent the presence of an inert gas such nitrogen or argon. The bubbles of the inert gas such as nitrogen or argon are moved into the solvent in the operation of the single crystal growth to form a large bubble and when the bubble is broken, smooth growth of the single crystal is prevented.

    [0031] It is preferable to gradually heat and cool at a rate of less than 30°C per minute at the initiation and completion of the calcination in order to prevent thermal cracking of the molded mixture.

    [0032] In the process of the present invention wherein the molded mixture for R3M5O12 is dissolved in the molten solvent and the single crystal of R3M5O12 is formed on the seed, the radiation convergence type floating zone method is employed in order to prevent a contamination with impurities and to increase the speed of the single crystal growth and to give uniform distribution of the components and to decrease the defects.

    [0033] The floating zone method used in the process of the present invention means that the rod for the product is rotated and fed from the higher position into the high temperature zone maintaining the temperature higher than the melting point of the rod, and the seed is rotated in the reverse direction and fed from the lower position and both the rod and the seed are contacted at the molten zone under the condition having no other support for the floating zone and then, both the rod and the seed are moved downwardly at a constant speed whereby the rod is dissolved into the molten solvent and the single crystal is formed on the seed from the molten solvent. The high temperature zone is maintained stably.

    [0034] The high temperature zone maintaining the temperature being higher than the melting point of the rod in the single crystal growth apparatus for the floating zone method should be maintained at higher than 1,450°C of the melting point of the solvent for 3 to 15 mm depending upon the diameter of the rod for R3M5O12.

    [0035] The length of the high temperature zone to be maintained higher than 1,450°C is not preferably longer or shorter than the range. The temperature distribution except near the high temperature zone is not critical.

    [0036] The single crystal growth apparatus used in the process of the present invention should have an equipment for sealing the single crystal growth part from the atmosphere and varying the condition of the environment as desired.

    [0037] The radiation convergence type floating zone method means the floating zone method wherein the stable high temperature zone is formed by the convergence of radiation from the light source at a high temperature by a mirror or a lens.

    [0038] The floating zone method of the present invention has the feature that the composition of the rod for R3M5O12 is different from that of the solvent. This is different from the conventional floating zone method.

    [0039] That is, the molten zone is formed by adhering a small amount of the molten solvent at the lower edge of the rod for R3M5O12. In this step, the molten solvent can be adhered on the top of the seed or on both of the lower edges of the rod for R3M5O12 and the top of the seed. The amount of the molten solvent is preferably that of a semi-spherical size having the diameter of the rod for R3M5O12. When the molten solvent is adhered on both of them, the amount of the molten solvent is preferably that of each semi-spherical size having the diameter of the rod or the seed. The molten solvent forms the floating zone by contacting the rod for R3M5O12 with the seed through the molten solvent.

    [0040] The seed can be any kind of solid which is resistant to high temperature and inert to the solvent and it is preferably a part of the calcined rod for R3M.012 especially the single crystal of R3M5012.

    [0041] The single crystal growth speed using the rod for R3M5O12, the solvent and the seed in the floating zone method is equal to the downward feeding speed of the rod and the seed. The single crystal of R3M5O12 is formed at a speed of greater than 0.1 mm per hour. The speed is preferably greater but it is preferably less than 10 cm per hour especially less than 8 mm per hour, optimumly in a range of 1 to 4 mm per hour. When it is too slow, the efficiency for producing the single crystal of R3M5O12 is lowered and the cost is increased.

    [0042] In order to prevent the formation of ferrous oxide in the resulting single crystal and to maintain the minimum electrical conductivity in the grown single crystal of R3M5O12, the oxygen pressure in the environment is maintained at at least 1.01 x 10-z bar (at least 10-2 atm). The oxygen pressure is preferably higher and especially in a range of 1.01 to 101 bar (1 to 100 atm.).

    [0043] When the resulting single crystal is used instead of the calcined rod for R3M5O12 in the production of the single crystal of R3M5O12, the single crystal is uniformly dissolved in the molten solvent whereby the recrystallization of the single crystal of R3M5O12 on the seed is stable and the single crystal having high quality can be obtained.

    [0044] In the specification the single crystal of R3M5O12 having high quality means a single crystal having a width of ferromagnetic resonance absorption of less than 5 Oe at room temperature though it is affected by the content of AI or Ga component.

    [0045] In accordance with the process of the present invention, the single crystal of R3M5O12 having high purity and uniform distribution of the components can be obtained at lower cost in comparison with the single crystal of R3M5O12 obtained by the conventional method.

    [0046] The single crystal of R3M5O12 obtained by the process of the present invention can be used as a magnetic material for microwaves which is the main use of those obtained by the conventional method. It also can be used in the other fields of magnetic materials such as spinel type ferrite, etc. as it is remarkably low in cost.

    [0047] The present invention will be further illustrated by examples.

    Example 1


    Single crystal growth of Y3Fe4.5Al0.5O12



    [0048] Y203 (purity of greater than 99.9%), Fe203 (purity of greater than 99.9%) and A1203 (purity of greater than 99.9%) in powdery forms were mixed at molar ratios of 3.0:4.5:0.5 as the mixture for Y3Fe4.5Al0.5O12 and at molar ratios of 0.17:0.95:0.05 as the mixture for the solvent.

    [0049] Each mixture was ground with acetone in a mortar to obtain each of two types of mixtures of fine powder having an average diameter of 1 µm.

    [0050] In a thin rubber tube having a diameter of 11 mm, about 12 g of each mixture was charged and both ends of the rubber tube were sealed. The rubber tube was inserted in a mold having an inner diameter of 11.5 mm and the mixture was molded under a pressure of 1 metric ton/cm2 for about 1 minute in an oil pressure type hydraulic apparatus.

    [0051] Each rod having a diameter of about 8 mm and a length of about 80 mm prepared by the molding step was calcined in a vertical type electric furnace at 1,550°C for the product and at 1,400°C for the solvent.

    [0052] The cracking of the rods caused by rapid heating and quenching was prevented by taking 1 hour for inserting and discharging the rod.

    [0053] The rod for the product of Y3Fe4.5Al0.5O12 having a diameter of about 6.5 mm and a length of about 60 mm was fixed on an upper rotary shaft for product of a floating zone single crystal growth apparatus employing infrared radiation convergence method. The rod for solvent having a diameter of about 7 mm and a length of about 20 mm was fixed on a lower rotary shaft for seed crystals. Oxygen 1.01 bar (1 atm) was fed into a crystal growth chamber partitioned from the ambient by a fused quartz tube to purge air and the heating operation was initiated. Oxygen was fed at a linear speed of 0.6 cm per second near the floating zone. The edge of the rod for solvent was adjusted to the position imparting highest temperature in a single crystal growth apparatus. When the edge was melted by the heating, the temperature was kept in constant and the rod for Y3Fe4.5Al0.5O12 was shifted downwardly into contact with the rod for solvent at the molten part. Then, the rod for solvent was cut out so as to leave suitable amount of the rod for solvent at the lower edge of the rod for Y3Fe4.5Al0.5O12. The rod for solvent was removed from the apparatus while cutting the radiation. A sintered rod of Y3Fe4.5Al0.5O12 having a diameter of 6.5 mm and a length of 20 mm as a seed crystal was fixed on the lower rotary shaft instead of the rod for solvent.

    [0054] The solvent adhered at the lower edge of the rod for Y3Fe4.5Al0.5O12 was melted by heating it. The seed crystal was adjusted to contact with the solvent and was contacted with the rod for product through the molten part. The seed crystal and the rod for product were respectively rotated at a speed of 30 rpm in opposite direction each other until completing the crystal growth. The condition for imparting suitable size of the molten part was maintained by finely controlling the temperature and the gap between the rod for product and the seed crystal. Then, both of them were shifted downwardly at a constant speed of 2.0 mm/hr to form a single crystal of Y3Fe4.5Al0.5O12 on the seed crystal. Polycrystalline product was initially formed but after the growth for 10 to 15 mm, the product had a sectional view of single crystal.

    [0055] When the rod for Y3Fe4.5Al0.5O12 was substantially consumed, the single crystal was cut out from the rod for product and was cooled to obtain a rod of single crystal of Y3Fe4.5Al0.5O12 having a diameter of 6 mm and a length of 40 mm.

    Example 2


    Single crystal growth of Y3Fe4AlO12



    [0056] Y201 (purity of greater than 99.9%), Fe203 (purity of greater than 99.9%) and A1201 (purity of greater than 99.9%) in powdery forms were mixed at molar ratios of 3.0:4.0:1.0 as the mixture for Y3Fe4AlO12 and at molar ratios of 0.17:0.9:0.1 as the mixture for the solvent.

    [0057] Each mixture was ground with acetone in a mortar to obtain each of two types of mixtures of fine powder having an average diameter of 1 µm.

    [0058] In accordance with the process of Example 1, the two types of the mixtures were treated to obtain a rod of single crystal of Y3Fe4AlO12 having a diameter of 6 mm and a length of 40 mm.

    [0059] The resulting cylindrical single crystal was sliced in parallel to the growth direction and the sectional surface was polished and observed by a microscope to find no ununiform part.

    Example 3


    Single crystal growth of Y3Fe4.5Al0.5O12 (high quality)



    [0060] The single crystal obtained by the process of Example 1 was used and recrystallized in accordance with the process of Example 1 to obtain a single crystal having a diameter of 6 mm and a length of 40 mm having high quality.

    [0061] A part of the resulting single crystal was cut out and was polished to form a spherical ball having a diameter of 0.5 mm and a width of ferro-magnetic resonance absorption of the ball was measured to result 1.8 Oe.

    Example 4


    Single crystal growth of Y3Fe4.5Ga0.5O12



    [0062] Y203 (purity of greater than 99.9%), Fe203 (purity of greater than 99.9%) and Ga2O3 (purity of greater than 99.9%) in powdery forms were mixed at molar ratios of 3.0:4.5:0.5 as the mixture for Y3Fe4.5Ga0.5O12 and at molar ratios of 0.17:0.95:0.05 as the mixture for the solvent.

    [0063] Each mixture was ground with acetone in a mortar to obtain each of two types of mixtures of fine powder having an average diameter of 1 µm.

    [0064] In accordance with the process of Example 1, the two types of the mixtures were treated to obtain a rod of single crystal of Y3Fe4.5Ga0.5O12 having a diameter of 6 mm and a length of 40 mm.

    [0065] The resulting cylindrical single crystal was sliced in parallel to the growth direction and the sectional surface was polished and observed by a microscope to find no ununiform part.

    Example 5


    Single crystal growth of Y3Fe4GaO12



    [0066] Y203 (purity of greater than 99.9%), Fe203 (purity of greater than 99.9%) and Ga203 (purity of greater than 99.9%) in powdery forms were mixed at molar ratios of 3.0:4.0:1.0 as the mixture for Y3Fe4GaO12 and at molar ratios of 0.17:0.9:0.1 as the mixture for the solvent.

    [0067] Each mixture was ground with acetone in a mortar to obtain each of two types of mixtures of fine powder having an average diameter of 1 µm.

    [0068] In accordance with the process of Example 1 ,sihe two types of the mixtures were treated to obtain a rod of single crystal of Y3Fe4GaO12 having a diameter of 6 mm and a length of 40 mm.

    [0069] The resulting cylindrical single crystal was sliced in parallel to the growth direction and the sectional surface was polished and observed by a microscope to find no ununiform part.

    Example 6


    Single crystal growth of Y2.5Nd0.5Fe5O12



    [0070] Y203 (purity of greater than 99.9%), Nd103 (purity of greater than 99.9%) and Fe203 (purity of greater than 99.9%) in powdery forms were mixed at molar ratios of 2.5:0.5:5.0 as the mixture for Y2.5Nd0.5Fe5O12 and at molar ratios of 0.14:0.03:1.0 as the mixture for the solvent.

    [0071] Each mixture was ground with acetone in a mortar to obtain each of two types of mixtures of fine powder having an average diameter of 1 µm.

    [0072] In accordance with the process of Example 1, the two types of the mixtures were treated to a rod of single crystal of Y2.5Nd0.5Fe5O12 having a diameter of 6 mm and a length of 40 mm.

    [0073] The resulting cylindrical single crystal was sliced in parallel to the growth direction and the sectional surface was polished and observed by a microscope to find no ununiform part.


    Claims

    1. A process for preparing a single crystal of an yttrium-iron garnet solid solution of the composition R3M5O12, wherein R represents Y which may be partly substituted by other rare earth elements and M represents Fe (III) which may be partly substituted by AI and/or Ga with the exception of Y3Fe5O12, at a single crystal growth rate of greater than 0.1 mm/h characterized in that the floating zone method is used, whereby, between an upper downwardly fed rotating rod of a mixture for the product and a lower downwardly moved counter rotating seed, a solvent zone is maintained by radiation convergence heating under an oxygen pressure of at least 1.01 x 10-2 bar (at least 10-2 atm.), whereby the composition of the solvent differs from that of the rod and is defined by a molar ratio of the M-component to the R-component of from 1:0.1 to 1:0.3 and in the presence of AI and/or Ga by a ratio of

    in the range of 1:1.5 to 1:2.5, wherein x represents Al2O3 and/or Ga203 and wherein MS and MC symbolize the molar concentration in the solvent and in the solid solution, respectively.
     
    2. A process according to claim 1, characterized by a molar ratio of the yttrium-oxide containing R-component to the ferric-oxide containing M-component of from 2.5:5.0 to 3.5:5.0 in the rod comprising the mixture for the product.
     
    3. A process according to one of claims 1 or 2, characterized in that a rod of the mixture for the product with a bulk density of more than 80% of the true density is used.
     


    Ansprüche

    1. Verfahren zur Herstellung eines Einkristalls einer festen Lösung eines Yttrium-Eisen-Granats der Zusammensetzung R3M5O12, wobei R für Y steht, welches teilweise durch ein anderes seltenes Erdelement substituiert sein kann und wobei M für Fe(III) steht, welches teilweise durch AI und/oder Ga substituiert sein kann, ausgenommen Y3Fe5O12 mit einer Einkristall-Wachstumsrate von mehr als 0,1 mm/h, dadurch gekennzeichnet, daß das Schwimmzonenverfahren angewendet wird, bei dem zwischen einem oberen abwärtsbewegten, rotierenden Stab aus einem Gemisch für das Produkt und einem unteren abwärtsbewegten, in Gegensinn rotierenden Kristallkeim eine Lösungsmittelzone aufrechterhalten wird, und zwar durch Strahlungskonvergenzbeheizung unter einem Sauerstoffdruck von mindestens 1,01 ×10-2 bar (mindestens 10-2 atm), wobei die Zusammensetzung des Lösungsmittels sich von der Zusammensetzung des Stabes unterscheidet und definiert ist durch ein Molverhältnis der M-Komponente zur R-Komponente von 1:0,1 bis 1:0,3 und, im Falle der Anwesenheit von AI und/oder Ga, durch ein Verhältnis von

    im Bereich von 1:1,5 bis 1:2,5, wobei x für Al2O3 und/oder Ga2O3 steht und wobei MS und M° die molare Konzentration im Lösungsmittel bzw. in der festen Lösung symbolisieren.
     
    2. Verfahren nach Anspruch 1, gekennzeichnet durch ein Molverhältnis der das Yttriumoxid enthaltenden R-Komponente zu der das Eisen-III-Oxid enthaltenden M-Komponente im Bereich von 2,5:5,0 bis 3,5:5,0 in dem Stab aus einer Mischung für das Produkt.
     
    3. Verfahren nach einem der Ansprüche 1 oder 2, dadurch gekennzeichnet, daß ein Stab aus einer Mischung für das Produkt mit einer scheinbaren Dichte von mehr als 80% der wahren Dichte verwendet wird.
     


    Revendications

    1. Procédé de préparation d'un monocristal d'une solution solide de grenat d'yttrium-fer ayant la composition R3M5O12 où R représente Y qui peut être partiellement remplacé par d'autres éléments de terres rares et M représente Fe (III) qui peut être partiellement substitué par AI et/ou Ga, à l'exception de Y3Fe5O12, à une vitesse de croissance du monocristal de plus de 0,1 mm/h, caractérisé en ce qu'il consiste à mettre en oeuvre la technique de la zone de flottation, technique selon laquelle on maintient, entre une tige supérieure rotative progressant vers le bas et formée d'un mélange pour le produit et un germe inférieur progressant vers le bas et tournant dans le sens opposé, une zone de solvant par chauffage par convergence de rayonnements sous une pression d'oxygène d'au moins 1,01 x 10-2 bar (au moins 10-2 atm) de sorte que la composition du solvent diffère de celle de la tige et soit définie par un rapport molaire du composant M au composant R allant de 1:0,1 à 1:0.3 et en présence de AI et/ou Ga dans un rapport de

    allant de 1:1,5 à 1:2,5, rapports dans lesquels x représente Al2O3 et/ou Ga2O3 alors que Ms et M° symbolisent les concentrations molaires dans le solvant et dans la solution solide, respectivement.
     
    2. Procédé selon la revendication 1, caractérisé en ce que le rapport molaire du composant R contenant de l'oxyde d'yttrium au composant M contenant de l'oxyde ferrique peut aller de 2,5:5,0 à 3,5:5,0 dans la tige constituée par le mélange pour le produit.
     
    3. Procédé selon la revendication 1 ou 2, caractérisé en ce que la tige constituée par le mélange pour le produit présente une densité apparente de plus de 80% de la densité vraie.